Background: Maxillary first premolar with wide MOD cavity more susceptible to fracture. The aim of this study was to assess the influence of cavity design for cusp coverage on the fracture resistance of weakened maxillary first premolar restored with CAD/CAM hybrid ceramic versus nanohybide composite. Materials and Methods: Fifty six intact maxillary first premolars of approximately comparable sizes were divided into seven groups eight for each: Group A: Intact teeth (control group); Group B: teeth prepared for MOD inlay; Group C: teeth prepared for MOD onlay covering the lingual cusp; Group D: teeth prepared for MOD covering buccal and lingual cusps ,the previous three groups indirectly restored with nanohybrid composite (3M ESPE Z 250 XT); Group E,F,G prepared with the same design as group B, C, D respectively and restored with CAD/CAM hybrid ceramic (VITA ENAMIC). Results: An axial compression test was used to measure the fracture strength of experimented teeth. The readings were analyzed statistically by t-test, one way ANOVA and LSD, then the mode of fracture had been examined. The results showed that sound teeth in group (A) had more fracture resistance values than all experimental groups and the difference were highly significant with group (B, E, F, G).When the influence of cavity design tested among composite groups it showed highly significant difference between group (B) and (C)and the highest fracture resistance value was for group(C), whereas the influence of cavity design among Enamic groups showed highly significant difference between group (E) and (G) the highest fracture resistance value was for group(E).T-test between similar designs showed non-significant difference between MOD groups and highly difference between other groups. Conclusions: Cusp coverage increased the fracture resistance of composite groups but result in non-restorable fracture, while Enamic total onlay presented promising fracture resistance with favorable mode of fracture. Key words: Fracture resistance, CAD/CAM, hybrid ceramic, VITA ENAMIC, nanohybrid composite, cusp coverage.
Background: Restoration of root canal treated teeth with a permanent restoration affect in the success of endodontically treated teeth. This in vitro study was performed to evaluate and compare the fracture strength of endodontically treated teeth restored by using custom made zirconium posts and cores, prefabricated carbon fiber, glass fiber and zirconium ceramic posts. Materials and method: Forty intact human mandibular second premolars were collected for this study and were divided into five groups. Each group contains 8 specimens: Group1: Teeth restored with Carbon Fiber Posts; Group2: Teeth restored with Glass Fiber Posts; Group3: Teeth restored with Zirconium Ceramic prefabricated Posts; Group4: Teeth restored with Zirconium Posts
... Show MoreBackground:The demand for esthetic orthodontic appliances is increasing so that the esthetic orthodontic archwires were introduced. This in vitro study was designed to evaluate the surface roughness offiber-reinforced polymer composite (FRPC) archwires compared to coated nickel-titanium (NiTi) archwires immersed in artificial saliva. Materials and Methods:Three types of esthetic orthodontic archwires were used: FRPC (Dentaurum), Teflon coated NiTi (Dentaurum) and epoxy coated NiTi (Orthotechnology). They were round (0.018 inch) in cross section and cut into pieces of 15 mm in length.Forty pieces from each type were divided into four groups; one group was left at a dry condition and the other three groups were immersed in artificial saliva (
... Show MoreBackground: This study was conducted to assess the effects of various beverages on the shear bond strength of light-cured orthodontic composite used to bond stainless steel orthodontic brackets on human teeth and to determine the site of bonding failure of this material. Materials and Methods: Fifty extracted human premolars were selected and randomly divided into five equal groups each with 10 teeth according to the beverage type (Control, One Tiger, Milk, Green tea and Coffee). After bonding, the teeth were immersed in specific beverages for 5 minutes twice daily with equal intervening intervals then washed and stored in distilled water at 37º C for the reminder of the day. The process was carried out for 30 days. The samples were then
... Show MoreABSTRACT Purpose: the aim of this in vitro study was to compare the marginal gap and internal fitness between single crowns and the crowns within three-unit bridges of zirconium fabricated by CAD-CAM system. Materials and methods: A standard model from ivoclar company was used as a pattern to simulate three-units bridge (upper first molar and upper first premolar) as abutments used to fabricate stone models, eight single crowns for premolar and eight of three units bridges. Crowns and bridges fabricated by CAD-CAM system were cemented on their respective stone models then sectioned at the mid-point buccolingaully and misiodistaly and examined under stereomicroscope. Result: the marginal gap in premolar crowns and premolar within bridge we
... Show MoreBackground: Prophylaxis methods are used to mechanically remove plaque and stain from tooth surfaces; such methods give rise to loss of superficial structure and roughen the surface of composites as a result of their abrasive action. This study was done to assess the effect of three polishing systems on surface texture of new anterior composites after storage in artificial saliva. Materials and methods: A total of 40 Giomer and Tetric®N-Ceram composite discs of 12 mm internal diameter and 3mm height were prepared using a specially designed cylindrical mold and were stored in artificial saliva for one month and then samples were divided into four groups according to surface treatment: Group A (control group):10 specimens received no surfa
... Show MoreBackground: White spot lesions are esthetic problems caused by subsurface enamel demineralization that seen as white opacity. Aim of the study: This study aimed to evaluate and to compare the color change after the treatment of the white spot lesions with resin nϔtrton and micro abrasion. Materials and Methods: rtϔ white spot lesions were generated on 48 premolar teeth by the use of a demineralization solution. The teeth were randomly divided using the Diagnodent into three study groups (16 teeth for each group) depending on the depth of the induced lesions: outer enamel, inner enamel and outer dentine. Then each group was fatherly subdivided into two groups (8 teeth for each group) the ϔrst group was treated wit
... Show MoreABSTRACT Background: One of the challenges to use chlorhexidine is its effect on the amount of microleakage after restoration; however, use of the materials with antibacterial properties after tooth preparation and before restoration has been widespread. The objective of this, in-vitro, study was to evaluate the influence of consepsis (chlorhexidine gloconate disinfectant) application on microleakage in class II cavities restored with light cured composite using universal adhesive system; etch and rinse technique –self etch technique. Materials and Methods: Forty class II cavities were prepared on mesial and distal surfaces of 20 non-carious mandibular third molars. The cavities were divided into four groups; (n =10 for each group).
... Show MoreBackground: Lack of durability of the bond of the dental adhesive systems to tooth structure is one of the most important problems in tooth colored restorative work. This in vitro study was performed to evaluate the effect of 2% chlorhexidine gluconate(CHX) on dentin bond strength by using total etch adhesive system at twenty-four hours and three months of water storage. Material and methods:A flat dentin surface was prepared for forty sound human maxillary premolar teeth which were acid etched with 36% phosphoric acid gel after being divided randomly into four groups of ten teeth each according to storage time and CHX application, theCHX was applied for 60 seconds before adhesive application for groups I and III which were tested after twe
... Show MoreBackground: This in vitro study was carried out to evaluate the effects of various veneering dentin ceramic thicknesses and repeated firings on the color of lithium disilicate glass-ceramic (IPS e.max Press) and zirconium-oxide (IPS ZirCAD) all-ceramic systems, measured by clinical spectrophotometers (Easyshade Advance 4.0) . Materials and methods: The 72specimens cube-shaped have the dimension of about 11 mm in width, 14 mm in length, 1mm in thickness, these cores divided into 3 groups according to the type of material each group have (24)core specimens. Each group had been divided into three sub-groups (each having 8 specimens) according to veneering with dentin ceramic thicknesses: as 0.5, 1, or 2 mm (n=8). IPS e.max press and ZirCAD c
... Show More