The structural, optical and electrical properties of ZnS films prepared by vacuum evaporation technique on glass substrate at room temperature and treated at different annealing temperatures (323, 373, 423)K of thickness (0.5)µm have been studied. The structure of these films is determined by X-ray diffraction (XRD). The X-ray diffraction studies show that the structure is polycrystalline with cubic structure, and there are strong peaks at the direction (111). The optical properties investigated which include the absorbance and transmittance spectra, energy band gab, absorption coefficient, and other optical constants. The results showed that films have direct optical transition. The optical band gab was found to be in the range to (2.96-3.06)eV with increasing annealing temperatures. The electrical properties of these films have been studied, it was observed that D.C conductivity at room temperature decreases with the increase of annealing temperatures, and the mechanism of conductivity occurs in two ranges of temperature, from Hall measurements the conductivity for all samples of ZnS films is n-type.
Copper selenide (Cu2Se) thin films were prepared by thermal evaporation at RT with thickness 500 nm. The heat-treating for (400 &500) K for the absorber layer has been investigated. This research includes, studying the structural properties of X-ray diffraction (XRD) that show the Cu2Se thin film (Cubic) and has a polycrystalline orientation prevalent (220). Moreover, studying the effect of annealing on their surface morphology properties by using Atomic Force Microscopy AFM. Optical properties were considered using the transmittance and absorbance spectra had been recorded when wavelength range (400 - 1000) nm in order to study the absorption coefficient and energy gap. It was found that these films had allowed direct transitio
... Show MoreIn this paper, we used two monomers, 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) and m,m'-diaminobenzophenone (m, m’-DABP), to produce polyamide acid and then converted it to polyimide (PI). The effects of phosphoric acid (H3PO4) molarity (1, 2, and 3 M) on the structural, thermal, mechanical, and electrical characteristics of the polyimides/polyaniline (PI/PANI) nanocomposites were studied. Two sharp reflection peaks were developed by the addition of PANI to PI. When 3 M H3PO4 is added, the crystalline sharp peak loses some of its intensity. The complex formation of PI/PANI-H3PO4 was confi
... Show MoreIn this paper the effect of nonthermal atmospheric argon plasma on the optical properties of the cadmium oxide CdO thin films prepared by chemical spray pyrolysis was studied. The prepared films were exposed to different time intervals (0, 5, 10, 15, 20) min. For every sample, the transmittance, Absorbance, absorption coefficient, energy gap, extinction coefficient and dielectric constant were studied. It is found that the transmittance and the energy gap increased with exposure time, and absorption. Absorption coefficient, extinction coefficient, dielectric constant decreased with time of exposure to the argon plasma
Thin films of tin disulphide SnS2 with different thicknesses (2500,4000,5000)A0 have been prepared by chemical spray pyrolises technique on substrate of glass with temperature (603)K . The effect of thickness on the optical properties of SnS2 has been studied.the optical study that includes the absorptance and transmittance spectra in the wavelength range (300900)nm demonstrated that the value of absorption coefficient (α) ) was greater than (104 cm-1) the electronic transitions at the fundamental absorption edge were of the indirect kind whether allowed and forbidden . Absorption edge shift slightly towards higher wave length.The value of energy gaps (Eg) for all the films prepared are decreased with inc
... Show MoreCdSe quantum dots possess a tuning energy gap which can control gap values according to the size of the quantum dots, this is made the material able to absorb the wavelengths within visible light. A simple model is provided for the absorption coefficient, optical properties, and optical constants for CdSe quantum dots from the size 10nm to 1nm with the range of visible region between (300-730) nm at room temperature. It turns out that there is an absorption threshold for each wavelength, CdSe quantum dots begin to absorb the visible spectrum of 1.4 nm at room temperature for a wavelength of 300 nm. It has been noted that; when the wavelength is increased, the absorption threshold also increases. This applies to the optical propertie
... Show MoreTin oxide films (SnO2) of thickness (1 ?m) are prepared on glass substrate by post oxidation of metal films technique. Films were irradiated with Nd:YAG double frequency laser of wavelength (532 nm) pulses of three energies (100, 500, 1000) mJ. The optical absorption, transmission, reflectance, refractive index and optical conductivity of these films are investigated in the UV-Vis region (200-900) nm. It was found that the average transmittance of the films is around (80%) at wavelength (550 nm) and showed high transmission (? 90 %) in the visible and near infrared region. The absorption edge shifts towards higher energies, which is due to the Moss-Burstien effect and it lies at (4 eV). The optical band gap increased with increasing of ene
... Show MoreThin films of Zinc Selenide ZnSe have been prepared by using thermal evaporation in vacuum technique (10-5Torr) with thickness (1000, 2700, 4000) A0 and change electrode material and deposited on glass substrates with temperature (373K) and study some electrical properties at this temperature . The graphs shows linear relation between current and voltage and the results have shown increases in the value of current and electrical conductivity with increase thickness and change electrode material from Aluminum to Copper
Study the effect of doping V2O5 on polymers poly vinyl alcohol ( PVA), poly vinyl pyrrolidone (PVP) on the optical and structural properties for film prepared by using Casting method at thickness( 300±20)nm ,All the materials dissolved in distilled water by magnetic mixer for one hour .The optical parameters measured by using UV-VIS spectrometer ,and the structural parameters measured by X-ray diffraction .when measured the energy gap found that the value was decreases from 4.6 eV to 2.98 eV with doping .The refractive index ,extinction coefficient ,absorption coefficient ,real and imaginary dielectric constants of (PVA/PVP) are increasing with doping by V2O5 and wit
... Show MoreAlloy of (HgTe) has been prepared succesful in evacuated qurtz ampoule at pressure 4×10-5torr, and melting temperature equal to 823K for five days. Thin films of HgTe of thickness 1μm were deposited on NaCl crystal by thermal evaporation technique at room temperature under vacuum about 4×10-5torr as well as investiagtion in the optical porperties included (absorption coefficient , energy gap) of HgTe films and The optical measurements showed that HgTe film has direct energy gap equal to 0.05 eV. The optical constants (n, k, εr, εi) have been measured over will range (6-28)μm.
This work describes, selenium (Se) films were deposited on clean glass substrates by dc planar magnetron sputtering technique.The dependence of sputtering deposition rate of Se film deposited on pressure and DC power has been studied. The optimum argon pressure has range (4x10-1 -8x10-2 )mbar. The optical properties such as absorption coefficient (α) was determined using the absorbance and transmission measurement from UnicoUV-2102 PC spectrophotometer, at normal incidence of light in the wavelength range of 200-850 nm. And also we calculated optical constants(refractive index (n), dielectric constant (εi,r), and Extinction coefficient (κ) for selenium films.