In this work, (Cu1-xAgx)2ZnSnSe4 (CAZTSe) alloys with various silver content (x= 0.0, 0.1and 0.2) have been prepared by reacting their high purity elements (Cu, Ag, Zn, Sn and Se) in an evacuated quartz tube under pressure of 10 -3Torr. The composition of the prepared alloys was determined by energy dispersive X-ray spectroscopy (EDXS) analysis, the results were close to the theoretical values. CAZTSe thin films with a thickness of 800 nm were deposited by thermal evaporation technique on glass substrates at room temperature (RT) with a deposition rate of 0.53nm/sec. Similarly, CdS thin films were deposited with a thickness of 100 nm on the same substrates at RT with a deposition rate of 0.3nm/sec from ready-made CdS alloy powder. All prepared thin films were annealed at temperatures of 373K and 473K under vacuum (10-3Torr) for 1h. X-ray analysis showed that all CAZTSe alloys and their thin films were polycrystalline and have the tetragonal structure with preferential orientation in the (112) direction, while all thin CdS films were polycrystalline and have the hexagonal structure with preferential orientation in the (002) direction. The scanning electron microscopy (SEM) technique was used to study the surface morphology of all prepared CAZTSe films, while the atomic force microscopy (AFM) technique was used to study the surface topography of all prepared CAZTSe and CdS films. SEM results revealed that CAZTSe films had uniform surface features with irregular sized grains, while AFM results showed that the surface roughness and the average grain size of CAZTSe and CdS thin films increased with increasing Ag content for CAZTSe thin films and annealing temperature for CAZTSe and CdS thin films. The absorbance and transmittance spectra for CAZTSe and CdS thin films were recorded in the wavelength ranges of (400-1100) nm and (350- 1100) nm, respectively. Optical measurements showed that all CAZTSe and CdS thin films have a direct energy gap (Eg) that decreased with increasing silver content for CAZTSe thin films and annealing temperature (Ta) for both types of prepared thin films, so it decreased from 1.73 eV to1.5 eV when x content increased from 0.0 to 0.2 and decreased from 1.5 eV to1.46 eV and from 2.47 eV to 2.38 eV when Ta increased from RT to 473K for CAZTSe thin films with x content equal to 0.2 and CdS thin films, respectively. Optical constants such as extinction coefficient, refractive index and dielectric constant were calculated for all prepared thin films. The measurements of the electrical properties for prepared films showed that the D.C electrical conductivity (σd.c) increased with increasing Ag content for CAZTSe thin films and annealing temperature for both types of thin films. So the electrical conductivity changed from 1.1276*10-2 (Ω.cm)-1 to 28.9266*10-2 (Ω.cm)-1 when x changed from 0.0 to 0.2 and changed from 28.9266*10-2 (Ω.cm)-1 to 57.4599*10-2 (Ω.cm)-1 and from 4.0476*10-4 (Ω.cm)-1 to 9.4227*10-4 (Ω.cm)-1 when Ta changed from RT to 473K for CAZTSe thin films with Ag content equal to 0.2 and CdS thin films, respectively. The prepared thin films have two activation energies (Ea1 & Ea2) in the temperature ranges of (318-488)K and (313-443)K for CAZTSe and CdS films, respectively. The results of Hall effect for CAZTSe thin films showed that all films were of acceptor type and the concentration of holes in them decreased with increasing silver content and annealing temperature, while CdS thin films were of donor type and the concentration of electrons in them increased with increasing annealing temperature. In this research, solar cells were fabricated from CdS/CAZTSe/Si structurThe C-V measurements revealed that all prepared heterojunctions were of the abrupt type and the junction capacitance and carrier concentration reduced while the width of depletion region and the built-in potential increased with increasing the silver content and annealing temperature. The current-voltage characteristics under dark condition of CAZTSe heterojunctions showed that both the ideality factor and saturation current decreased with increasing Ag content and annealing temperature. While,The current-voltage characteristics under dark condition of CAZTSe heterojunctions showed that both the ideality factor and saturation current decreased with increasing Ag content and annealing temperature. While, the current-voltage measurements under illumination showed that the performance of heterojunction solar cell improved with increasing Ag content and annealing temperature. The result indicated that the prepared solar cell with 0.2 Ag content and 473K annealing temperature exhibited the highest efficiency (η = 2.827%) compared to other prepared solar cells
New designs of solar using ray tracing program, have been presented for improved the performance and the out put power of the silicon solar cell, as well as reducing the cost of system working by solar energy. Two dimensional solar concentrator (Fresnel lenses) and three dimensional concentrators (parabola dish and cassegrain) were used as concentrator for photovoltaic applications (CPV). The results show that the performance efficiency and out power for crystalline silicon solar cells are improved.
Aqueous root extract has been used to examine the green production of silver nanoparticles (AgNPs) by reducing the Ag+ ions in a silver nitrate solution. UV-Vis spectroscopy, X-ray diffraction, field emission scanning electron microscopy, and Fourier transform infrared spectroscopy (FTIR) were used to analyze the produced AgNPs. The AgNPs that were created had a maximum absorbance at 416 nm, were spherical in form, polydispersed in nature, and were 685 nm in size.The AgNPs demonstrated antibacterial efficacy against Escherichia coli and Staphylococcus. The dengue vector Aedes aegypti's second instar larvae were very susceptible to the AgNPs' powerful larvicidal action.
In this work, a (CdO)0.94:(In2O3)0.06 film was developed on a glass substrate using Q- switching pulse laser beam (Nd:YAG; wavelength 1064 nm). The quantitative elemental analysis of the (CdO)0.94:(In2O3)0.06 thin film was achieved using energy dispersive X- ray diffraction (EDX). The topological and morphological properties of the deposited thin film were investigated using atomic force microscope (AFM) and field emission scan electron microscopy (FESEM). The I-V characteristic and Hall effect of (CdO)0.94 :(In2O3)0.06 thin films were used to study the electrical properties. The gas sensor prope
... Show MoreThe multi-dentate Schiff base ligand (H2L), where H2L=2,2'-(((1,3,5,6)-1-(3-((l1-oxidaneyl)-l5-methyl)-4-hydroxyphenyl)-7-(4-hydroxy-3-methoxyphenyl)hepta-1,6-di ene-3,5-diylidene)bis(azaneylylidene))bis(3-(4-hydroxyphenyl)propanoic acid), has been prepared from curcumin and L- Tyrosine amino acid. The synthesized Schiff base ligand (H2L) and the second ligand 1,10-phenanthroline (phen) are used to prepare the new complexes [Al(L)(phen)]Cl, K[Ag(L)(phen)] and [Pb(L)(phen)]. The synthesized compounds are characterized by magnetic susceptibility measurements, micro elemental analysis (C.H.N), mass spectrometry, molar conductance, FT-infrared, UV-visible, atomic absorption (AA), 13C-NMR, and 1H-NMR spectral studies. The characterization of the
... Show MoreThe objective of this research is to study the possibility of reducing the reflectivity of the front surface of a silicon cell (Si / Si) by using a theoretical design for a single-layer Antireflection Coatings with a thickness of one quarter of the design wavelength. Then, Mathematical programs in MATLAB (10) were designed to study the quantitative efficiency of the cell as a function of the change in the particle size of the coating within the range (400 - 700 nm) wavelength of the visible state of the vertical and oblique state at the (45°) angle. (Ge) was used as an anti-reflective material. It was found that the highest quantitative efficiency was (96.9004%) at design wavelength (λ0= 550 nm)
... Show MoreIn this research (100* 40* 4 cm) solar cell panel was used in Baghdad at autumn season (2010), to get best solar cell panel angles experimentally, and then a mirror (40*50 cm) is use to concentrate incident sunlight intensity on a panel. At first case we get (Tilt angle ?P =60°and Surface Azimuth angle ?P =36°E) is the best angles and other case, we add a mirror at angle = 120° at bottom of panel, then we get output power (27.48watt) is bigger than without using a mirror (25.16watt). We can benefit from these cases in variety applications.
The synthesis , characterization and mesomorphic behaviour of new Nacyl , thiourea and imidazole derivatives which derived from corresponding Schiff bases are reported. All the synthesized compounds which contain flexible methylene group in the centre of the molecule did not show any liquid crystalline properties . The derivatives of N- acyl [III]e and thiourea [VI]e which contain biphenyl and all compounds with one phenyl in the centre of the molecule display liquid crystalline behaviour .While the imidazoles did not show any liquid crystalline properties except [V]b [V]e with biphenyl in the centre of the molecule . All th
... Show More