Objective. This study aimed to evaluate and compare the force degradation of two types of elastomeric chains following different periods of immersion in zinc-containing mouthwashes. Materials and Methods. Four hundred and forty pieces of Elasto-Force and Super Elasto-Force elastomeric chains were divided into two control and eight experimental groups. The pieces were stretched to 25 mm on pins mounted on an acrylic block and stored in distilled water at 37°C. The experimental groups were immersed in four different types of mouthwash for one minute twice a day throughout the test period. Ten continuous thermocycles per day between cold and hot water baths (5–55°C) were carried out. Forces were measured at six-time intervals (initial, 24 hours, 1, 3, 6, and 8 weeks). The mean force was calculated and compared among different elastomeric chains, mouthwashes, and times using the t-test and one-way ANOVA test followed by Tukey’s HSD test. The level of significance was set at 0.05. Results. Both types of elastomeric chains had significant force degradation over time (74–79% at 8 weeks). The Super Elasto-Force generated a higher force level than the Elasto-Force elastomeric chain at all time points. SmartMouth Clinical DDS mouthwash had a significantly lower effect on force degradation than other mouthwashes with no significant difference compared to control groups. Conclusions. Depending on these results: there is no clinically significant difference between both types of elastomeric chains, although Super Elasto-Force delivered a higher force level. The pH of the mouthwashes could play a role in force degradation over time, rather than other ingredients including zinc. The SmartMouth mouthwash had the minimum effect on force degradation of elastomeric chains, followed by Halita, Listerine Total Care Zero, and Breath Rx, respectively.
Background: Orthodontic therapy often causes external root resorption. Serum vitamin D (VD) level is important for tooth mineralization and bone remodeling. This study aimed to test the impact of vitamin D (VD) supplements on bone and root remodelling in a vitamin D (VD) deficient rat model following orthodontic retention. Methods and Material: 30 male Wistar rats were divided into three groups: a control group of 10 rats and two experimental groups of 10 rats each with vitamin D deficiency (VDD) induced by a VD-free diet for 21 days. And a third group with VD supplementAll groups received orthodontic active treatment using a modified orthodontic appliance that applied 50 gm of force for 14 days to move the maxillary right first mol
... Show MoreBackground: This study was performed to determine the effect of aging of different types of composite material restorations on: Shear bond strength (SBS) to light cure and no mix chemical cure orthodontic adhesives with sapphire bracket and the debonding failure sites. Materials and methods: One hundred forty four composite disks were made from three different composite resin materials which are: 3M Filtek Z250, 3M filtek Z350 and 3M Valux plus, each group with (48) disks each, then according to the duration of storage each group was subdivided into two equal groups one of them stored for one day and the other was stored for one month, then each group was further subdivided into two equal subgroups with (12) disks each one bonded with ligh
... Show MoreBackground:Plant-derived compounds have action alongside Gram-positive and Gram-negative bacteria and numerous compounds, inhibit efflux pumps and hence have become known as efflux pump inhibitors. Clarithromycin is a macrolide antibiotic used to treat pharyngitis, tonsillitis, acute maxillary sinusitis and acute bacterial exacerbation of chronic bronchitis the antibacterial range is the similar as erythromycin but it is active against Mycobacterium avium complex, M.leprae and atypical mycobacteria. The in vitro antibacterial activity results of different boswellic acid compounds discovered alpha keto-boswellic acid (AKBA) to be the preponderance potent antibacterial compound alongside Gram-positive pathogens, but it showed no significant a
... Show MoreIntroduction: We aimed to assess the impact of adhesive and wires types on the tensile bond strength of fixed lingual retainers. Methods: A total of 160 intact bovine teeth were collected, cleaned, stored in 25% sodium hypochlorite, and randomly assigned to two groups based on the adhesive type: a two-step adhesive and a one-step adhesive. Each group was further divided into four subgroups based on the type of lingual retainer wire, which included (A) 8-strand braided stainless steel wire, (B) three-strand titanium retainer wire, (C) stainless steel chain, and (D) fiber-reinforced retainer. A tensile bond strength test was conducted using a universal testing machine at a controlled speed of 10 mm/min. Result: The 8-strand braided stainles
... Show MoreBackground: Prophylaxis methods are used to mechanically remove plaque and stain from tooth surfaces; such methods give rise to loss of superficial structure and roughen the surface of composites as a result of their abrasive action. This study was done to assess the effect of three polishing systems on surface texture of new anterior composites after storage in artificial saliva. Materials and methods: A total of 40 Giomer and Tetric®N-Ceram composite discs of 12 mm internal diameter and 3mm height were prepared using a specially designed cylindrical mold and were stored in artificial saliva for one month and then samples were divided into four groups according to surface treatment: Group A (control group):10 specimens received no surfa
... Show MoreABSTRACT Background:Hydrogen absorption and related degradation in the mechanical properties of Ni-Ti based orthodontic wires has been demonstrated following exposure to fluoride prophylactic agents. This study was designed to investigate the effects of three fluoride containing agents on the load deflection characteristics of heat activated nickel titanium arch wires during unloading phase. Material and method: Eighty specimens of heat activated nickel titanium arch wires were obtained from Ortho Technology Company, half of which had a 0.016 inch round and 0.019x0.025 rectangular. Ten specimens from both wire size were immersed in one of the tested fluoride prophylactic agents (neutral sodium fluoride gel, stannous fluoride gel or phos-flu
... Show MoreThis study aimed to incorporate hydroxyapatite nanoparticles (nHA) or amorphous calcium phosphate nanoparticles (nACP) into a self-etch primer (SEP) to develop a simplified orthodontic bonding system with remineralizing and enamel preserving properties.
nHA and nACP were incorporated into a commercial SEP (Transbond™ plus) in 7% weight ratio and compared with the plain SEP as a control. Shear bond strengths (SBS), enamel damage, and adhesive remnant index (ARI) scores were evaluated at 24 h
Background: evaluate the effects of three different intracoronal bleaching agents on the shear bond strengths (SBS) and failure site of stainless steel and monocrystalline (sapphire) orthodontic brackets bonded to endodontically treated teeth using light cured orthodontic adhesive in vitro. Materials and methods: Eighty extracted sound human upper first premolars were selected, endondontically treated and randomly divided equally (according to the type of the brackets used) into two main groups (n = 40 per group). Each main group were subdivided (according to the bleaching agent used) into four subgroups 10 teeth each; as following : control (un bleached) group, hydrogen peroxide group (Hp) 35%, carbamide peroxide group (CP) 37% group and s
... Show More