This paper focused on the stone matrix asphalt (SMA) technology that was developed essentially to guard against rutting distress. For this procedure, fibers play a racy role in stabilizing and preventing the drain down problem caused by the necessity of high binder content coupled with their strengthening effect. A set of specimens with cylindrical and slab shapes were fabricated by inclusions jute, polyester, and carbon fibers. For each type, three contents of 0.25%, 0.5%, and 0.75% by weight of mixture were added by lengths of 5, 7.5, and 10 mm. The prepared mixtures were tested to gain the essential pertained parameters discriminated by the values of drain down, Marshall quotient, rut depth, and dynamic stability. It has appeared that the fibers rate of 0.5% and 7.5 mm length is much appropriate to yield the best performance of modified mixtures. At these values, carbon fibers recorded the highest increase level of rutting resistance and dynamic stability by 53% and 100%, respectively while, jute fibers exhibited the lowest improvement by only 34% and 63%, respectively; nevertheless, they produced mixtures having the lowest drain down value. Regarding the index of plastic stiffness, polyester fibers embedded mixtures occupied the first rank of increasing by 38%.
Moisture damage is a primary mode of distress occurring in hot mix asphalt (HMA) pavements in Iraq. Because of the loss of bond, or stripping, caused by the presence of moisture between the asphalt and aggregate, which is a problem in some areas and can be severe in some cases, it is requires to evaluate the design asphalt mixture to moisture susceptibility. Many factors such as aggregate characteristics, asphalt characteristics, environment, traffic, construction practices and drainage can contribute to stripping. Asphalt concrete mixes were prepared at their optimum asphalt content by superpave system and then tested to evaluate their engineering properties, which include tensile strength, resilient modulus, and perman
... Show MoreThe action of high repeated trucks load associated with dramatically elevated ambient temperatures leads to the most harmful distress in asphalt pavements occurred in Iraq known as rutting. Essentially, it is produced from the accumulation of irrecoverable strains, which mainly occurred in the asphalt layers. That visually demonstrated as a longitudinal depression in the wheel paths as well as small upheavals to the sides. Poly Phosphoric Acid (PPA) has been used as a means of producing modified asphalt binders and the interest to use it has increased in recent years. The PPA provides modified asphalt binder, which is relatively cheaply produced compared to polymer-modified asphalt. In this paper, PPA was used by three-percentages 1
... Show MoreOne of the major problems facing the road construction engineer is the collapsible granular soil which may be used for embankment construction. Problems appears when such compacted soil come in touch with water, it exhibits cracking and uncontrolled settlement. Collapsible soils are defined as any unsaturated soil that goes through a radical rearrangement of practice and great loss of volume upon wetting, with or without additional loading. An attempt has been made in this investigation to stabilize the collapsible soil of Nasiriya with asphalt emulsion. Specimens of pure and asphalt emulsion stabilized soil have been prepared using optimum fluid content and tested. The first group of specimens of (60x60x20) cm have been tested for direct s
... Show MoreIn order to get better understanding of asphalt pavement performance, asphalt from five Iraqi refineries (Qayarah, Nassiriyah, Baiji, Samawah and Daurah) were analyzed into five chemical fractions including asphaltenes, polar compounds, first acidaffins, second acidaffins and saturated hydrocarbons where the last four fractions called maltenes. Polar compounds /saturated hydrocarbons ratio (PC/S) and the ratio of the reactive to the unreactive components of the maltenes fraction (durability rating) parameters were determined. The study showed that Baiji asphalt has the best durability over other asphalts, while Qayarah asphalt is considered to have the least durability grade. These results confirm the correlation of the chemical composit
... Show MoreIn this work, some mechanical properties of the polymer coating were improved by preparing a hybrid system containing Graphene (GR) of different weight percentages (0.25, 0.5, 1, and 2wt%) with 5wt% carbon fibres (CF) and added to a polymer coating by using casting method. The properties were improved as GR was added with further improvement on adding 5wt% of CF. The impact strength of acrylic polymer with GR increases with increasing weight ratio of GR; maximum value was obtained when the polymer coating was incorporated with 1wt% GR and 5wt% CF. The impact strength of acrylic polymer with GR and GR/CF composites incorporated with GR at 1wt% and CF at 5wt%. Hardness increase with increasing weight ratio of Gr and a significant imp
... Show MoreThis research is devoted to study the effect of different in weight percentage of Sio2 particles and glass fibers (5, 10, 15, 20) wt. % on the wear rate epoxy resin. The results show that the value of hardness increase with the increase for the weight percentage of reinforcing particles and fibers, while the wear rate decrease with the increase the load level of the reinforcing particles and fibers . The largest value of the hardness, and the lowest value of the wear rate for epoxy reinforced with 20% of SiO2, the wear rate increase in general with increasing the applied load.
In this research a study of the effect of quality, sequential and directional layers for three types of fibers are:(Kevlar fibers-49 woven roving and E- glass fiber woven roving and random) on the fatigue property using epoxy as matrix. The test specimens were prepared by hand lay-up method the epoxy resin used as a matrix type (Quick mast 105) in prepared material composit . Sinusoidal wave which is formed of variable stress amplitudes at 15 Hz cycles was employed in the fatigue test ( 10 mm )and (15mm) value 0f deflection arrival to numbers of cycle failure limit, by rotary bending method by ( S-N) curves this curves has been determined ( life , limit and fa
... Show MoreIn this study, experimental mortar combinations with 1% micro steel fibers, were examined to create geopolymer mortars. To test the effect of the fibers on the mortar's resistance, the geopolymer mortar was designed with various proportions of more environmentally friendly materials fly ash and slag. The percentage of fly ash by weight was 50, 60, and 70% of the slag. The best results were obtained when a 50:50 ratio of fly ash and slag were mixed with 1% micro steel fibers. The results showed that the mixtures containing fibers performed better in the considered tests (toughness index, ductility index, and resilience index). In the impact resistance test, the mixture contained 50% fly ash by weight of the slag with a temperature of
... Show MoreHot mix recycling of asphalt pavements is increasingly being used as one of the major rehabilitation methods by various highway agencies. Besides general savings in costs and energy expended, it also saves our natural resources and environment. Recycling process presents a sustainable pavement by using the old materials that could be reclaimed from the pavement; these materials could be mixed with recycling agents to produce recycled mixtures. The important expected benefits of recycling process are the conservation of natural resources and reduction of environmental impact. The primary objectives of this work are evaluating the Tensile and Shear Properties of recycled asphalt concrete mixtures, In addition to the
... Show More