The corrosion behavior and corrosion inhibition of α-brass (65.3% Cu, 34.4% Zn and others 0.3%) in 0.6 mol.dm-3 NaCl solution have been investigated using potentiostatic polarization technique, the main results obtained were expressed in terms of corrosion (Ec) and corrosion current (ic). The research was performed in neutral and slightly acidic media [pH=7 and pH=4] over the temperature range (288-318)K. It was found that the rate of corrosion increases with the increase of acidity and the increase of temperature. The rate of corrosion increased with the increase of temperature in conformity with Arrhenius equation. Values of activation energy (Ea*), pre-exponential factor (A) and entropy of activation (∆S*) have been derived for the corrosion process. Also the thermodynamic quantities (∆G, ∆S and ∆H) have been determined for the process. The inhibition effect of thiourea on the corrosion of α-brass in chloride solution was studied, and it was found that the addition of thiourea to the chloride solution caused a decrease in the values of corrosion current density and changed to some extent the values of kinetic parameters. The values of (Ea) increases in the presence of thiourea, this means that the decrease of the concentration of thiourea
Galvanic corrosion of stainless steel 316 (SS316) and carbon steel (CS) coupled in 5% wt/v sulfuric acid solution at agitation velocity was investigated. The galvanic behavior of coupled metals was also studied using zero resistance ammeter (ZRA) method. The effects of agitation velocity, temperature, and time on galvanic corrosion current and loss in weight of both metals in both free corrosion and galvanic corrosion were investigated. The trends of open circuit potential (OCP) of each metal and galvanic potential (Eg) of the couple were, also, determined. Results showed that SS316 was cathodic relative to CS in galvanic couple and its OCP was much more positive than that of CS for all investigated ranges of
... Show MoreThe present study develops an artificial neural network (ANN) to model an analysis and a simulation of the correlation between the average corrosion rate carbon steel and the effective parameter Reynolds number (Re), water concentration (Wc) % temperature (T o) with constant of PH 7 . The water, produced fom oil in Kirkuk oil field in Iraq from well no. k184-Depth2200ft., has been used as a corrosive media and specimen area (400 mm2) for the materials that were used as low carbon steel pipe. The pipes are supplied by Doura Refinery . The used flow system is all made of Q.V.F glass, and the circulation of the two –phase (liquid – liquid ) is affected using a Q.V.F pump .The input parameters of the model consists of Reynolds number , w
... Show MoreDrilling solutions can be considered as an intricate mixture comprising of number of chemical additives which aid specific needs such as controlling the rheological properties and reducing corrosion. Inhibitors are substances that are added in small concentrations to corrosive environment to decrease the corrosion. Their applications can be found in drilling equipments. The effect of adding Zinc Sulphate and Carboxymethyl Cellulose to study their influence on the corrosion of carbon steel in Bentonite mud has been evaluated using Weight Loss Technique. This study focuses on determining rheological properties and corrosion characteristics. Results show CMC and ZnSO4 work as inhibitors when added to the Bentonite with inhibition
... Show MoreIn this work, electrochemical process was presented to polymerized eugenol on Gr.2 and Gr.5 titanium alloys before and after treated by Micro Arc Oxidation (MAO), where Gr.2 is commercial pure titanium and Gr.5 is Ti-6Al-4V dental alloys. The deposited layers were characterized by scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDS), X-ray diffraction (XRD), and Fourier transform infrared spectroscopy (FTIR). The adhesion strength of polymeric thin-film was estimation by using pull-off adhesion test and the result was the adhesion strength of PE was (1.23 MPa) on Gr.2 before MAO and increase to (1.98 MPa) on Gr.2 after MAO treatment. The corrosion behavior of Gr.2 and Gr.5 alloy in artificial saliva environment at
... Show MoreThe galvanic corrosion of the (Cu - Fe), (Cu - Zn) and (Fe - Zn) couples have been investigated in 3.5% NaCl solution, 40ºC, different velocities (Re = 5000, 10000 and 15000) and different area ratio’s of cathode to anode (AR= 0.5,1 and 2), by using commercial metal pipe (cylindrical tube).The Zero Resistance Ammeter has been used to measure the galvanic current (Ig) and galvanic potential (Eg) with time. The galvanic current density increases with increasing velocity (Re) and the area ratio (AR). The galvanic potential (Eg) is shifted to less negative with increasing velocity (Re) and the area ratio (AR). A statistical relations for the galvanic current density and galvanic potential as a function of (Re). and the area ratio had been
... Show MoreThe petroleum industry, which is one of the pillars of the national economy, has the potential to generate vast wealth and employment possibilities. The transportation of petroleum products is complicated and changeable because of the hazards caused by the corrosion consequences. Hazardous chemical leaks caused by natural disasters may harm the environment, resulting in significant economic losses. It significantly threatens the aim for sustainable development. When a result, determining the likelihood of leakage and the potential for environmental harm, it becomes a top priority for decision-makers as they develop maintenance plans. This study aims to provide an in-depth understanding of the risks associated with oil and gas pipeli
... Show MoreInternal curing is a method that has been advised to decrease the primary age cracking, mainly of concrete mixes using low (water to cementitious materials - w/cm) ratios corresponding to the self-compacting concrete-(SCC). This research aims to study the effect of the internal curing using saturated lightweight aggregate- (LWA) on the steel reinforcing corrosion in SCC. In this research, crushed bricks or thermostone were partially replaced by (20%) by the weight of sand and volumetrically measured. The results showed that the steel reinforcement of internally cured concrete showed a slight increase in corrosion up to 300 days of exposure to the saline solution (containing 3.5% NaCl). The ability of using the crushed bricks or thermostone
... Show MoreInternal curing is a method that has been advised to decrease the primary age cracking, mainly of concrete mixes using low (water to cementitious materials - w/cm) ratios corresponding to the self-compacting concrete-(SCC). This research aims to study the effect of the internal curing using saturated lightweight aggregate- (LWA) on the steel reinforcing corrosion in SCC. In this research, crushed bricks or thermostone were partially replaced by (20%) by the weight of sand and volumetrically measured. The results showed that the steel reinforcement of internally cured concrete showed a slight increase in corrosion up to 300 days of exposure to the saline solution (containing 3.5% NaCl). The ability of using the crushed bricks or thermostone
... Show MoreThe inhibitive action of pomegranate peel as a plant source the corrosion of carbon-steel in phosphoric acid solutions was studied using the weight-loss method. Organic compounds present in natural materials are successfully used to reduce the rate of corrosion because they are cheap, renewable and effective. The results showed that the inhibition potency was enhanced with increasing increasing the amount of the inhibitor and the immersion time but it decreased with the increase of the concentration of the acid solution. The results also revealed a gradual increase in the corrosion rate with the increase of temperature, while the corrosion protection efficiency and surface coverage decreased.