In this research, the mechanical properties of natural rubber blends in different proportions (70:30, 85:15, 100: 0 55:45 and phr) was studied through the use of two types of fillers (carbon black and titanium dioxide Nano) which show through tests conducted on the prepared models that increase fillers content which leads to improve the tensile properties (tensile strength, elastic modulus, elongation, hardness and compressibility). As shown by the results that the presence of polypropylene (PP) in the mix combination works to reduce the degree of intumescent and increase its content in the composition of mixtures which leads to get a great resistance to chemicals (acids, bases and oils).
Objective: Dental caries is a chronic infectious disease that is prevalent worldwide in all age groups. Numerous attempts have been made to develop conservative approaches to halt caries progression and restore enamel defects. This study aimed to investigate the effect of applying grape seed extract and chicken eggshell extract on the microhardness of demineralized enamel in permanent teeth. Methods: Forty-eight sound upper first premolars were used. Following demineralization with the demineralizing solution for 96 hours, they were distributed into four groups consistent with the treatment agent used: group A was treated with casein phosphopeptide amorphous calcium phosphate (as a control group), group B was treated with grape se
... Show MoreA polycrystalline PbxS1-x alloys with various Pb content ( 0.54 and 0.55) has been prepared successfully. The structure and composition of alloys are determined by X-ray diffraction (XRD), atomic absorption spectroscopy (AAS) and X-ray fluorescence (XRF) respectively. The X-ray diffraction results shows that the structure is polycrystalline with cubic structure, and there are strong peaks at the direction (200) and (111), the grain size varies between 20 and 82 nm. From AAS and XRF result, the concentrations of Pb content for these alloys were determined. The results show high accuracy and very close to the theoretical values. A photoconductive detector as a bulk has been fabricated by taking pieces of prepared alloys and polished chemic
... Show MoreGlass Ionomer Cement (GIC) is one of the important dental temporary filing materials. The aim of this study is to evaluate the effect of adding 3, 5 and 7 wt. % of TiO2 microparticles to conventional GIC powder (Riva Self Cure) on mechanical properties and its effect on absorption and solubility processes. TiO2 particles additives improved compressive strength and biaxial flexural strength, where the compressive strength increased with increasing in the added ratio, while the highest value of the biaxial flexural strength was at 3 wt.%. The addition of TiO2 particles improved the surface Vickers microhardness values, with highest value at 5 wt. %. On other hand TiO2 addition im
... Show MoreBackground: Poly (methylmethacrylate) is not ideal in every aspect and has disadvantages such as insufficient surface hardness, increase water sorption and poor impact resistance and the latter being the primary cause of fracture of denture base resins. The aim of this study was to evaluate the effect of addition of silanized nano- hydroxyapatite (HA) on some properties of heat cured acrylic denture base material. Materials and methods: HA nano particles were first silanized with ï§MPS (tri methacryloxypropyletrimethoxy silane coupling agent) then ultrasonicated with methylmethacrylate (monomer) to disperse agglomerated nano particles and mixed with polymer. 2% by wt of HA nano particles was selected as the best concentration that add
... Show MoreIn this research,we are studied impact strength, bending and compression strength of composites including the epoxy resin as a matrix , with gawaian red wood flour ,Russian white wood flour ,glass powder and rock wool fibers as reinforcement materials with volume fraction (20%) for all samples,and compared them in different conditions of temperatures. The results have shown that the impact strength increased with the reinforcement with (particles and fibers),and at high temperatures for all samples prepared,and also observed an increase in elasticity coefficient of epoxy composites filled with (different particles) and decreased in elasticity coefficient of epoxy com
... Show More(Cu1-x,Agx)2ZnSnSe4 alloys have been fabricated with different Ag content(x=0, 0.1, and 0.2) successfully from their elements. Thin films of these alloys have been deposited on coring glass substrate at room temperature by thermal evaporation technique under vacuum of 10-5Torr with thickness of 800nm and deposition rate of 0.53 nm/sec. Later, films have been annealed in vacuum at (373, and 473)K, for one hour. The crystal structure of fabricated alloys and as deposited thin films had been examined by XRD analysis, which confirms the formation of tetragonal phase in [112] direction, and no secondary phases are founded. The shifting of main polycrystalline peak (112) to lower Bragg’s angle as compared to Cu2ZnSnSe4 angle refers to incorpora
... Show MorePreparation of epoxy/ TiO2 and epoxy/ Al2O3 nanocomposites is studed and investigated in this paper. The nano composites are processed by different nano fillers concentrations (0, 0.01, 0.02 ,0.03, 0.04 ,0.05 ,0.07 and 0.1 wt%). The particles sized of TiO2,Al2O3 are about 20–50 nm.Epoxy resin and nano composites containing different shape nano fillers of (TiO2:Al2O3 composites),are shear mixing with ratio 1 to 1,with different nano hybrid fillers concentrations( 0.025 ,0.0 5 ,0.15 ,0.2, and 0.25 wt%) to Preparation of epoxy/ TiO2- Al2O3 hybrid composites. The mechanical properties of nanocomposites such as bending ,wearing, and fatigue are investigated as mechanical properties.
The aim of this research is to develop mechanical properties of a new aluminium-lithium-copper alloy. This alloy prepared under control atmosphere by casting in a permanent metal mould. The microstructure was examined and mechanical properties were tested before and after heat treatment to study the influence of heat treatment on its mechanical properties including; modulus of elasticity, tensile strength, impact, and fatigue. The results showed that the modulus of elasticity of the prepared alloy is higher than standard alloy about 2%. While the alloy that heat treated for 6 h and cooled in water, then showed a higher ultimate tensile stress comparing with as-cast alloy. The homogenous heat treatment gives best fatigue
... Show MoreBackground: Dental erosion is a common oral condition which results due to consumption of high caloric and low pH acidic food such as carbonated drinks and fruit juices. It is expected that these food types can cause irreversible damage to dental hard tissues and early deterioration of the dental restorations. So, this study aimed to evaluate and compare the erosive potential effects of orange fruit juice and Miranda orange drink on the microhardness of an orthodontic composite material. Materials and methods: Thirty discs with a thickness of 2 mm and a diameter of 10 mm were prepared from orthodontic bonding composite. The prepared discs were equally divided into three groups (n=10). Microhardness analysis was carried out both prior to
... Show MoreBark fiber has high potential use for composite reinforcement in biocomposite material. The aim of this study is the mechanical properties of Bark fiber reinforced polester composite with varying fiber weight fraction (0% , 5% , 10% , 20%, 30% and 40%) hand lay-up technique which was used to prepare the composite , specimens for tensile , flexural and impact test according to the ASTM D638 , ASTMD790 , and Iso-179. The over all results showed that the composite is reinforced with Bark fiber at weight (10%) higher mechanical properties , and the composite showed improved mechanical (Flexural).