CdSe thin films were deposited on glass sudstrate by thermal evaporation method with thickness of (300±25%) nm with deposition rate (2±0.1) nm/s and at substrate temperature at (R.T.). XRD analysis reveals that the structure of pure thin films are Hexagonal and polycrystalline with preferential orientation (002). In this research ,we study the effect of doping with (1,2,3)% Aluminum on optical energy gap of (CdSe) thin film . The absorption was studied by using (UV - Visible 1800 spectra photometer ) within the wavelength (300-1100) nm absorption coefficient was calculated as a function of incident photon energy for identify type of electronic transitions it is found that the type of transition is direct , and we calculated the optical energy gap before and after doping we found that the energy gap decreases after doping and absorption coefficient increases.
The effect of the annealing on the optical transmission , absorp tion coefficient,
dielectric constants (ε
r
),( ε
i
) ,Skin depth and the optical ener gy gap of (ZnO)x(CdO)1-x thin
films with (x=0.05) deposited on preheated glass substrates at a temperature of (450 C°) by
chemical pyrolysis technique were performed . These f ilms show direct allowed inter band
transition that influenced by annealing at ( 450 C°) for two hours . And it also found that the
optical ener gy gap has been increased fro m about (2.50 eV) before annealing to about (2.65
eV) after annealing , fro m the analysis of the absorp tion and transmission sp ectra in the
wavelength range (380-900nm) . The results show t
optical properties of pure poly(vinyl Alcohol) films and poly(vinyl Alcohol) doped with methyl red were study, different percentage prepared with constant thickness using casting technique. Absorption, Transmission spectra have been recorded in order to study the optical parameters such as absorption coefficient, energy gap, refractive index, Extinction coefficient and dispersion parameters were measured in the wavelength range (200-800)nm. This study reveals that the optical properties of PVA affect by increasing the impurity concentration.
The nonlinear optical properties response of nematic liquid crystal (6CHBT) and the impact of doping with two kinds of nanoparticles; Fe3O4 magnetic nanoparticles and SbSI ferroelectric nanoparticles have been studied using the non-linear dynamic method through z-scan measurement technique. This was achieved utilizing CW He-Ne laser. The pure LC and magnetic LC nanoparticle composite samples had a maximum absorption while the ferroelectric LC nanoparticle composite had a minimum absorption of the incident light. The nonlinear refractive index was positive for the pure LC and the rod-like ferronematic LC composite samples, while it was negative for the ferroelectric LC composite. The studying of the nonlinear optical
... Show MoreAlloys of Bi2[Te1-x Sex]3 were prepared by melting technique with different values of Se percentage (x=0,0.1,0.3,0.5,0.7,0.9 and 1). Thin films of these alloys were prepared by using thermal evaporation technique under vacuum of 10-5 Torr on glass substrates, deposited at room temperature with a deposition rate (12nm/min) and a constant thickness (450±30 nm). The concentrations of the initial elements Bi, Te and Se in the Bi2 [Te1-x Sex]3 alloys with different values of Se percentage (x), were determined by XRF,The morphological and structural properties were determined by AFM and XRD techniques. AFM images of Bi2[Te1-x Sex]3 thin films show that the average diameter and the average surface roughness inc
... Show MoreA thin CdS Films have been evaporated by thermal evaporation technique with different thicknesses (500, 1000, 1500 and 2000Å) and different duration times of annealing (60, 120 180 minutes) under 573 K annealing temperature, the vacuum was about 8 × 10-5 mbar and substrate temperature was 423 K. The structural properties of the films have been studied by X- ray diffraction technique (XRD). The crystal growth became stronger and more oriented as the film thickness (T) and duration time of annealing ( Ta) increases.
The electronic properties and Hall effect of thin amorphous Si1-xGex:H films of thickness (350 nm) have been studied such as dc conductivity, activation energy, Hall coefficient under magnetic field (0.257 Tesla) for measuring carrier density of electrons and holes and Hall mobility as a function of germanium content (x = 0–1), deposition temperature (303-503) K and dopant concentration for Al and As in the range (0-3.5)%. The composition of the alloys and films were determined by using energy dispersive spectroscopy (EDS) and X-ray photoelectron spectroscopy (XPS).
This study showed that dc conductivity of a-Si1-xGex:H thin films is found to increase with increasing Ge content and dopant concentration, whereas conductivity activati
In this work, As60Cu40-xSex thin films were synthesized, and the pulsed laser deposition method was used to study the effected partial replacement of copper with selenium. The electrical characteristics and optical characteristics, as indicated by the absorbance and transmittance as a function of wavelength were calculated. Additionally, the energy gap was computed. The electrical conductivity of the DC in the various conduction zones was calculated by measuring the current and voltage as a function of temperature. Additionally, the mathematical equations are used to compute the energy constants, electron hopping distance, tail width, pre-exponential factor, and density of the energy states in variation zones (densities of the energ
... Show MoreThe alloys of CdSe1-xTex compound have been prepared from their elements successfully with high purity (99.9999%) which mixed stoichiometry ratio (x=0.0, 0.25, 0.5, 0.75 and 1.0) of (Cd, Se and Te) elements. Films of CdSe1-xTex alloys for different values of composition with thickness(0.5?m) have been prepared by thermal evaporation method at cleaned glass substrates which heated at (473K) under very low pressure (4×10-5mbar) at rate of deposition (3A?/s), after that thin films have been heat treated under low pressure (10-2mbar) at (523K) for two hours. The optical studies revealed that the absorption coefficient (?) is fairly high. It is found that the electronic transitions in the fundamental absorption edge tend to be allowed direct tr
... Show MoreThin films of BhSe3 have being deposited on glass substrates of
about 80 - 172 ± 14 nm thickness from an aqueous solution bath at temperature 293 K for period 0.5 to 6.0 hours using alchemical bath deposition method .
The films are characterized by X-ray diffraction, X-ray
florescent techniques and optical transmittance spectra measurements in the rang 350 - 400 nm at 293 K. And shows that as deposited films are amorphous and a transition to polycrystalline state has taken place after annealing them at 373 K, for 30 minutes, But they will be dan1aged
... Show More