Thin film technology is one of the most important technologies
that have contributed to the development of semiconductors and their
applications in several industrial fields. The Iron Oxides (Fe20) and
(Co3O4) thin films and their applications are of importance, in that these
two materials are considered as important industrial materials, and used
in spectrally selective coating, temperature sensors, resistive heaters, and
photo cells.
Thin films of Iron Oxide (Fe20,), Cobalt Oxide (Co304) and
their mixtures in different ratios (75:25, 50:50, 25:75) were prepared by
the method of chemical spray pyrolysis deposition at different thicknesses
(77s t S200) nm on cover-glass substrates: thickness of (1) mm at
temperature (653)OK, and at temperature (753)oK for (one, and two) hour.
The nature of the thin-films
surfaces are examined by optical
microscopy, while the crystallinity of the compounds is examined by X
ray diffraction (XRD)
The results of KRD) have shown that the films of (Fe20,) and
(Co304) and their mixtures are of amorphous structure. Annealing
operations led to transition of the films' structure from the amorphous to polycrystalline state. These obtained results were found in
agreement with the American Standard for Testing Materials (ASTM).
Film thickness, and annealing time were investigated, the results show the
crystallite size increases with the increase of the thickness of the thin
film
The increase in the annealing time for more than one hour resulted
in the appearance of some peaks in diffraction spectrum of the prepared
films. This verifies that it is polycrystalline, and this increases the time to
organize itself in the crystalline lattice and decreases the crystalline
defect. This research also included the study of the optical properties of
the prepared samples by recording the absorption and transmission
spectrum over the spectral range (200-900 nm, the optical energy gap for
the allowed direct transition was evaluated. In general, the optical energy
gap decreases with increase of the film thickness percentage of (Co3O4)
in the sample, and it increases after annealing
The optical parameters are investigated and calculated such a
optical absorption coefficient, photon energy, and the width of localized
states too. It is found that the values of absorption coefficient the
increases with increasing percentage of (Co3O4)
The effect of thermal treatment on optical constants of pure PMMA and with addition (15 and 35) ml of coumarin at different temperatures (100, 110 and 120) C0 for 1 hour were investigated. Cast method used to prepares films of pure PMMA and PMMA with (15 and 35) of coumarin. UV/VIS spectrometer technique used to measure the absorption spectra for these films. The optical constant (absorption spectra and absorption coefficient) don’t changes after applied temperatures in pure PMMA film but the optical constant (absorption spectra and absorption coefficient) in PMMA with (15 and 35) ml of coumarin increased with applied temperatures. The optical energy gap of pure PMMA and PMMA with (15 and 35) ml of coumarin sl
... Show MoreDiamond-like carbon (DLC) homogeneous thin films were deposited from cyclohexane (Ccyclohexane (Ccyclohexane (Ccyclohexane (C cyclohexane (Ccyclohexane (Ccyclohexane (C cyclohexane (Ccyclohexane (C 6H12 ) liquid by using a plasma jet system which operates with alternating high voltage 7.5 which operates with alternating high voltage 7.5which operates with alternating high voltage 7.5which operates with alternating high voltage 7.5 which operates with alternating high voltage 7.5which operates with alternating high voltage 7.5which operates with alternating high voltage 7.5 which operates with alternating high voltage 7.5which operates with alternating high voltage 7.5 which operates with alternating high voltage 7.5which operates with al
... Show MoreZinc oxide (ZnO) nanoparticles were synthesized using a modified hydrothermal approach at different reaction temperatures and growth times. Moreover, a thorough morphological, structural and optical investigation was demonstrated using scanning electron microscopy (SEM), x-ray diffraction (XRD), ultra-violate visible light spectroscopy (UV-Vis.), and photoluminescence (PL) techniques. Notably, SEM analysis revealed the occurrence of nanorods-shaped surface morphology with a wide range of length and diameter. Meanwhile, a hexagonal crystal structure of the ZnO nanoparticles was perceived using XRD analysis and crystallite size ranging from 14.7 to 23.8 nm at 7 and 8 ℎ𝑟𝑠., respectively. The prepared ZnO samples showed good abso
... Show MoreThin filis have been prepared from the tin disulphide (SnS2 ), the pure and the doped with copper (SnS2:Cu) with a percentages (1,2,3,4)% by using ahemical spray pyrolysis techniqee on substrate of glass heated up to(603K)and sith thicknesses (0.7±0.02)?m ,after that the films were treated thermally with a low pressure (10-3mb) and at a temperature of (473K) for one hour. The influence of both doping with copper and the thermal treatment on some of the physical characteristics of the prepared films(structural and optical) was studied. The X-ray analysis showed that the prepared films were polycrystalline Hexagonal type. The optical study that included the absorptance and transmitance spectra in the weavelength range (300-900)nm
... Show MoreZnO nanostructures were synthesized by hydrothermal method at different temperatures and growth times. The effect of increasing the temperature on structural and optical properties of ZnO were analyzed and discussed. The prepared ZnO nanostructures were characterized by X-ray diffraction (XRD), UV–Vis. absorption spectroscopy (UV–Vis.), Photoluminescence (PL), and scanning electron microscopy (SEM). In this work, hexagonal crystal structure prepared ZnO nanostructures was observed using X-ray diffraction (XRD) and the average crystallite size equal 14.7 and 23.8 nm for samples synthesized at growth time 7 and 8 hours respectively. A nanotubes-shaped surface morphology was found using scanning electron microscopy (SEM). The optic
... Show MoreIn the present work, silver nanoparticles were prepared. Nonlinear optical properties and
optical limiting of silver nanoparticles were investigated.Standard chemical synthesis method was used at
diffrent weight ratio(0.038, 0.058 and 0.078) of silver nitrate. Several testing were done to obtain the
characteristics of the sample. Z-Scan experiments were performed using 30 ns Q-switched Nd:YAG
laser at 1064 nm and 532 nm at different intensities. The results showed that the nonlinear refractive
index is directly proportional to the input intensities, which caused by the self-focusing of the material.
In addition, the optical limiting behavior has been studied. The results showed that the sample could be
used as an opt
This paper reports the effect of Mg doping on structural and optical properties of ZnO prepared by pulse laser deposition (PLD). The films deposited on glass substrate using Nd:YAG laser (1064 nm) as the light source. The structure and optical properties were characterized by X-ray diffraction (XRD) and transmittance measurements. The films grown have a polycrystalline wurtzite structure and high transmission in the UV-Vis (300-900) nm. The optical energy gap of ZnO:Mg thin films could be controlled between (3.2eV and 3.9eV). The refractive index of ZnO:Mg thin films decreases with Mg doping. The extinction coefficient and the complex dielectric constant were also investigate.
InSb alloy was prepared then InSb:Bi films have been prepared successfully by thermal evaporation technique on glass substrate at Ts=423K. The variation of activation energies(Ea1,Ea2)of d.c conductivity with annealing temperature (303, 373, 423, 473, 523 and 573)K were measured, it is found that its values increases with increasing annealing temperature. To show the type of the films, the Hall and thermoelectric power were measured. The activation energy of the thermoelectric power is much smaller than for d.c conductivity and increases with increasing annealing temperature .The mobility and carrier concentration has been measured also.
In this research the electrical conductivity measurements were made on the amorphous InAs films prepared by thermal evaporation method in thickness 450 nm and annealed in different temperatures in the range (303- 573) K. The electrical conductivity (σ) showed a decreasing trend with the increasing annealing temperature, while the activation energies (Ea1, Ea2) showed an opposite trend, where the activation energies are increased with the annealing temperature.