Polymer composite materials were prepared by mixing epoxy resin with sand particles in three different grain size (150-300 ), (300-600 ) and (600- 1200) μm . The weight of epoxy was 15%, 20%, 25% and 30% of the total weight. Compression strength and flexural strength tests were carried out for the prepared samples .The percentages of epoxy resin at 20% wt and 25% wt showed best mechanical properties for all grain sizes .These percentages were adopted to fill the void between particles sand which have two different size ranges (150-600) μm and {(150-300) & (600-1200)} μm respectively to obtain more dense material. The results showed that the strength of polymer composite at 20% resin is higher than 25% resin. The sample which has maximum value for compression strength and flexural strength was reinforced with fibers (glass, polypropylene and alucobond waste) by weight 1% and 1.5% respectively of the weight of epoxy resin.
Background: The aim of this study was to evaluate the effect of thermo cycling and different pH of artificial saliva (neutral, acidic, basic) on impact and transverse strength of heat cure acrylic resin reinforced of with 5% silanated ZrO2 nano fillers. Materials and methods: 120 samples were prepared, 60 samples for impact strength test and another 60 samples for transverse strength test, for each test, samples were divided into two major groups (before and after thermo cycling), then each of these major groups were further subdivided into 3 subgroups according to the pH of prepared artificial saliva (neutral, acidic, basic). Charpy impact device was used for impact strength test and Flexural device was used for transverse strength test. R
... Show MoreBackground: Thermocycling simulates the temperature dynamics in the oral environment. This in vitro study done to measure and compare the effect of thermocycling on the shear bond strength of stainless steel and sapphire brackets bonded to human enamel teeth using light cured orthodontic adhesive and debonded at various time, and to measure adhesive remnant index after debonding. Materials and Methods: one-hundred-twenty extracted upper first premolars for orthodontic reason were used in this study; depending on weather thermocycled or not, the sample was divided into two main groups, then within each group 30 teeth were used for stainless-steel brackets (Bionic®) and for sapphire brackets (Pure®). Both groups were subdivided into three
... Show MoreBackground: In dentistry, dentist takes the advantages of soft lining materials due to the viscoelastic properties. The major problem is the adhesion of the soft liner with the denture base material. Materials and Methods: Heat cured of high impact acrylic resin specimens prepared with dimensions 75x13x13mm for shear bond strength test, soft lining material (Refit and Mollosil) with a 3-mm thickness and used to join each two acrylic blocks. Also four specimens with the same previous dimensions utilized for chemical and physical surface analysis. The specimens grouped as control (without plasma) and experiment (with oxygen plasma) treated high impact acrylic specimens. Results: Plasma treatment increased the shear bond strength for both Refi
... Show MoreNormal concrete is weak against tensile strength, has low ductility, and also insignificant resistance to cracking. The addition of diverse types of fibers at specific proportions can enhance the mechanical properties as well as the durability of concrete. Discrete fiber commonly used, has many disadvantages such as balling the fiber, randomly distribution, and limitation of the Vf ratio used. Based on this vision, a new technic was discovered enhancing concrete by textile-fiber to avoid all the problems mentioned above. The main idea of this paper is the investigation of the mechanical properties of SCC, and SCM that cast with 3D AR-glass fabric having two different thicknesses (6, 10 mm), and different layers (1,2 laye
... Show MoreThis work has been done with using of epoxy resin mixed with Granite powder were weighted by percent volume (5,10,15, and 20)%and then mixed with epoxy polymer to compose polymer composite. Hand lay-up technique is used in fabrication of the composite samples. Hardness test was carried out for the proper samples in both normal condition and after immersion in HCL (1 M and 2 M) solutions for periods ranging up to 10 weeks. After comparing the results between the polymer and their composite, the hardness increased with increasing Granite weight percent, it was found that Hardness were greater for the composites before immersion compared with their values after immersion.
The objective of this work was to determine and compare the physiological changes in some: blood components (packed cell volume and hemoglobin) and plasma biochemical parameters (glucose, total protein, albumin, cholesterol and triglycerides) under 3 day of different types of stress: water deprivation, starvation, overcrowding and handling stress. Twenty five male Wister rats weighted 100-120 gm, were divided randomly into five groups: control, water deprivation, starvation, overcrowding and handling stress. On the third day of stress the animals anesthetized for blood collection; the results of blood component revealed a significant increase in PCV and a significant decrease in Hb of water deprivation group and starva
... Show More