Background: Impression materials, impression trays, and poured stone cast have been said to be the main source of cross infection between patients and dentists. However, it was observed that disinfection of the impression is not performed systematically in routine dental practice. Disinfection of alginates either by immersion or spray technique was found to cause dimensional inaccuracies, although with proper disinfection of alginates there were small dimensional changes. A variety of fluoride releasing products designed for topical use is currently available. Following their use, varied amount of fluoride is systemically absorbed depending on the fluoride concentration and the manner of its use. The objective of this study was to evaluate the effect of addition (0%, 0.25%,0.5%,1%, 2%, 3%, 4% ) of (NaF) as a self-disinfection to alginate impression material powder and its effect on setting time, tear strength, dimensional change and accuracy of alginate impression materials. Materials and methods: A total No. of (700) specimen were used in this study.These specimens were divided into (5) main groups according to the tests used. Each of the four main groups contain (70) specimen divided into 7 subgroups (ten specimens to be tested for each (7)concentrations which is composed of six percentages of NaFwith alginate powder (0.25%,0.5%,1%, 2%, 3%, 4% )and one for control (0% NaF) , while the fifth group (Microbiological test) contain 420 specimen were divided between Streptococcus mutans and Candida albicans as (120) specimen for each one that was subdivided into three subgroups (specimens taken before impression casting, specimensafter pouring of alginate with stone andspecimens of stone were taken from the casts) in which it contain the same subgroups of the other concentrationsof (NaF) to test its efficacy against (Streptococcus mutans and Candida albicans). Results: Tear strength for all experimental impression materials was greater than those of the control products. There were no statistically significant differences between the dimensional change tests and also reproduction of detail test.With regard to setting time of the impressions, statisticallyreduction were seen between the control and experimental groups of alginate impression materials that contain (NaF). Self-disinfection of alginate impression material containing NaF showed a significant reduction in the count of cell forming unit of microorganisms immediately after impressions were made. Conclusion: In cooperation of specific concentrations of (NaF) as a disinfectant in alginate dental impression produced a significant reduction of contamination, also they caused non-significant effect on dimensional stability, detail reproduction and significant increase in tear strength. Therefore it is recommended as step in preventing cross contamination. Keywords: Alginate, NaF, Candida Albicans, streptococcus mutans.
In this study a polymeric composite material was prepared by hand
lay-up technique from epoxy resin as a matrix and magnesium oxide
(MgO) as a reinforcement with different weight fraction (5,10,15,
and 20)% to resin. Then the prepared samples were immersed under
normal condition in H2So4(1 M) solution, for periods ranging up to
10 weeks. The result revealed that the diffusion coefficient
decreasing as the concentration of MgO increase. Also we studied
Hardness for the prepared samples before and after immersion. The
result revealed that the hardness values increase as the concentration
of MgO increase, while the hardness for the samples after immersion
in H2SO4 dec
Background: The success and maintenance of indirect dental restorations is closely related to the marginal accuracy, which is affected by many factors like preparation design, using of different fabrication techniques, and the time of taking final impression and pouring it. The purpose of this in vitro study was to evaluate the effect of different pouring time of conventional impression on the vertical marginal gap of full contour zirconia crowns in comparison with digital impression technique. Materials and Methods: Forty sound recently extracted human permanent maxillary first premolar teeth of comparable size and shape were collected. Standardized preparation of all teeth samples were carried out to receive full contour zirconia crown re
... Show MoreBackground: The success and maintenance of indirect dental restorations is closely related to the marginal accuracy, which is affected by many factors like preparation design, using of different fabrication techniques, and the time of taking final impression and pouring it. The purpose of this in vitro study was to evaluate the effect of different pouring time of conventional impression on the vertical marginal gap of full contour zirconia crowns in comparison with digital impression technique. Materials and Methods: Forty sound recently extracted human permanent maxillary first premolar teeth of comparable size and shape were collected. Standardized preparation of all teeth samples were carried out to receive full contour zirconia crown re
... Show MoreSodium Dodecyle Sulphate (CH3(CH2)11SO4-Na+) solution was used as a secondary oil recovery by using a lab Model shown in figure-1. The effect of (solution concentration, temperature and salinity) on interfacial tension figure-2 and figure-3 and figure-4 respectively. The best values of these three variables, were taken (those values that give the lowest interfacial tension). Porosity, saturation, permeability were determined in the lab depending on Darcy law. Primary oil recovery was displaced by water until no more oil is obtained then sodium dodecyle sulphate solution was injected. The total oil recovery was 94.8% or 85.7% of the residual oil (secondary oil recovery) figure-5. This method was applied on Iraqi oil field and it gave resu
... Show MoreEP/ metal composites were prepared as adhesives between two steel rods. Epoxy resin (EP) was used as a matrix with metal as fillers (Al, Cu, Fe,).
The preparation method for tensile adhesion tests includes two steel rods with adhesive composites between the rods to measure adhesion strength Sad and adhesion toughness Gad.
Results of tensile adhesion tests show that EP/ metals composite have maximum strength Sad for certain weight percentage of metals 2.95 and 9MPa at 10% for EP/Al and EP/Cu composite and 8.2MPa at 40% for EP/Fe composites
The work was carried out in two stages. The first stage concerned
with study of silicon carbide (SiC) ratio (1.5, 2.5, 3.5, and 4.5 wt%)
effect on the Thermal conductivity of polyvinyl chloride (PVC); and
the second stage concerned with the UV – weatherizing (25, 50, and
75 hr), thermal aging (40, 50, and 60 °C), and rain- weatherizing (1,
2.5, and 4 hr) effect on the samples involved. Thermal conductivity
results proved that there was slight increase in thermal conductivity
by (SiC) loading; it increased from 0.17 W/m.K for PVC to 0.19
W/m.K for 4.5% SiC/PVC; where as it was systematically decreased
by UV- weatherizing, thermal aging, and rain- weatherizing. This
property is in a good agreement with gene
Background: The PMMA polymer denture base materials are low in thermal and strength properties. The aim of the study was to investigate the change in glass transition temperature, E-Moudulus and coefficient of thermal expansion of acrylic denture base material by addition of Al2O3, TiO2 and SiO2nano-fillers in 5% by weight. Materials and methods: The type of polymerization is free radical bulk polymerization. one hundred twenty (120) specimens were prepared , the specimens were divided into four groups according to the material had been added (one control and three for Al2O3, TiO2 and SiO2nanocomposite) each group was subdivided in to three groups according to the test had been done on it, the degree of transition (Tg) was measured by The d
... Show MoreNaturally available products have been used widely for centuries in handling human disease. The present study aimed to determine the effect of aluminum potassium sulfate addition into the soft liner on tensile strength and peel bond strength. The effect of aluminum potassium sulfate evaluated by two methods, first one include incorporation of KAL (SO4)2 into soft liner monomer in concentration (2%,3% by wt.) while the second method include immersion of soft liner specimens in solution of KAL(SO4)2 in concentration(5%,10% percent) during time periods (0,10 minutes). In conclusions, the results of current study encourage use KAL (SO4)2 within soft liner material
This study is a complementary one to an extended series of research work that aims to produce a thermodynamiclly stable asphalt –sulfur blend. Asphalt was physically modified wiht different percentages of asphaltenes , oxidized asphaltenes and then mixed with sulfur as an attempt to obtaine a stable compatible asphalt-sulfur blend. The homogeneneity of asphalt-asphaltenes[oxidized asphaltenes]-sulfur blends were studied microscopically and the results are prsented as photomicrographs. Generally more stable and compatible asphalt-sulfur blends were obtained by this treatment.