Background: The aim of the study was to investigate the effect of surface treatments of zirconia (grinding and sandblast with 50μm, 100 μm) on shear bond strength between zirconia core and veneering ceramic. Material and methods: Twenty-eight presintered Y-TZP ceramic specimens (IPS e.max ZirCAD, Ivoclar vivadent) were fabricated and sintered according to manufacturer’s instructions. The core specimens were divided randomly in to 4 groups, group 1: no surface treatment, group2: zirconia specimens were ground with silicon carbide paper up to1200 grit under water cooling, group3: zirconia specimens were ground and sandblast with 100 μm alumina, group 4: zirconia specimens were ground and sandblast with 50 μm alumina. Surface roughness of specimens were analyzed by surface profilometer, then veneering ceramic (IPS e.max ceramic, Ivoclar vivadent) was applied on the specimens& fired according to manufacturer’s instructions. All specimens were subjected to shear force in a universal testing machine at a crosshead speed of 1mm/min. The shear bond strength values were analyzed with one-way ANOVA; the fractured surfaces were examined with a stereo-microscope to observe the failure mode. Results: The mean of shear bond strength values in MPa were 24.75 for group 4, (17.72) for group 3, (17.68) for group2, (14.61) for group 1.The airborne-particle abrasion with 50μm group showed significantly higher bond strength than other groups. The airborne-particle-abraded with 100 μm group was not significantly different from grinding group. Conclusion: With limit of this study, the sandblast with 50 μm alumina was enhance the SBS between zirconia &veneering ceramic, and zirconia-veneering ceramic bonding is not only influenced by surface roughness. But also may be other factors.
Purpose: To evaluate the effect of different surface treatments on shear bond strength between dentin and IPS e.max lithium disilicate glass-ceramic. Materials and Methods: Eighteen extracted third molars were embeded in epoxy resin. The tooth was sectioned vertically in mesiodistal direction using a low speed hard tissue microtome. The buccal and lingual surfaces of each section were ground flat using 600 grit Silicone carbide paper. Eighteen ceramic discs consisted of lithium disilicate glass-ceramic were prepared with a diameter of 4.7mm and height of 2.2mm. The discs were divided in two groups (n=10): (1) IPS e.max treated with hydrofluoric acid and Monobond Plus (MBP) and (2) IPS e.max treated with Monobond Etch &Prime (MBEP). The toot
... Show MoreBackground: the aim of this study was to evaluate the effect of different surface acids treatments (37%phospjoric acid, 5%hydrofluoric acid, 1.23 acidulated phosphate fluoride) of feldspathic ceramic VITA 3D MASTER , and the effect of thermocycling on shear bond strength using a ceramic repair kit (ivoclar/vivadent). Material and Methods: sixty Nickel-Chromium metal base plates were prepared(9mm diameter,3mm depth) using lost wax technique, 2mm thick layer of ceramic(VITA 3D MASTER) fused to metal plates, all specimens were embedded in acrylic resin blocks except their examined surfaces and divided into 3 main groups 20 specimens each, Grp A: treatment with 37%phosphoric acid for 2 mins, Grp B: etching with 5% hydrofluoric acid for 2mins,
... Show MoreBackground: This study aimed to evaluate the effect of zirconia different surface treatments (primer, sandblast with 50μmAl2O3, Er,Cr:YSGG laser) on shear bond strength between zirconia surface and resin cement. Material and methods: Sixty presintered Y-TZP zirconia cylinder specimens (IPS e.max ZirCAD, Ivoclar vivadent) will be fabricated and sintered in high temperature furnace of (1500 C for 8 hours) according to manufacturer’s instructions to the selected size and shape of (5mm. in diameter and 6mm in height). All specimens were ground flat using 600.800.1000.1200, aluminum oxide abrasive paper to obtain a standardized surface roughness. Surface roughness values were then recorded in µm using surface roughness tester (profi
... Show MoreBackground: Separation and deboning of artificial teeth from denture bases present a major clinical and labortory problem which affect both the patient and the dentist. The optimal bond strength of artificial teeth with denture base reinforced with nanofillers and flexible denture bases and the effect of thermo cycling should be evaluated. This study was conducted to evaluate and compare the shear bond strength of artificial teeth (acrylic and porcelain) with denture bases reinforced by 5% Zirconium oxide nanofillers and flexible bases under the effect of different surface treatments and thermo cycling and comparing the results with conventional water bath cured denture bases. Material and methods: Two types of artificial teeth; acrylic and
... Show MoreBackground: Fracture of different types of acrylic denture base is a common problem associated with dental prosthesis. Studies suggested that the repair strength may be improved by several means including surface treatment with chemical agents. The aim of the study was to evaluate the effect of surface treatment with acrybond-bonding agent and monomer on fractured denture base in respect to transverse, tensile and shear bond strength and evaluation of the mode of failure by light microscope. Materials and methods: Two hundred seventy specimens were prepared and divided into 3 groups according to the material used (regular conventional, rapid simplified and high impact) heat cure acrylic. The specimen in each groups were prepared specificall
... Show More
The zirconia ceramic restoration (ZCR) is used as substitutes for the metal-ceramic restoration. Clinical studies demonstrating of ZCRs showed a high fracture incidence of veneering layer than metal-ceramic restorations. This attributed to the low bond strength of zirconia to veneering ceramic as a result of lacking of glass content in its matrix. Surface treatment was proposed to improve the bonding strength between zirconia and veneering ceramic. Several studies revealed that some treatment such as airborne particle abrasion (APA) is responsible for generating chipping of veneering ceramic. The study aimed to develop a new zirconia coatings to increase bonding strength between zirconia substrate and veneering porcelain. Three groups of 15
... Show MoreBackground and objectives: This study aimed at testing the effect of plastic sleeve or barrier, used to cover the guide of the light cure unit to prevent cross-infection, on the shear bond strength and site of bond failure of stainless steel and ceramic orthodontic brackets. Materials and methods: Forty orthodontic brackets; twenty stainless steel and twenty ceramic brackets bonded to forty extracted human maxillary first premolars using light cure adhesive cured with and without the use of a protective plastic barrier on the guide. Comparing the effect of this barrier on the shear bond strength and adhesive remnant index was performed using an independent t-test and Chi-square test. Results: The protective barrier had decreased the shear b
... Show More