Background:In this study,TiO2 layer was thermally grown as a diffusion barrier on CP Ti substrate prior to electrophoretic deposition of HA coatings, to improve the coating’s compatibility also macro and micro pores in nano Hydroxyapatite dual coatings were created and their effect on the bond strength between the bone and implant was evaluated. Materials and methods: Electrophoretic Deposition technique (EPD) was used to obtain coatings for each one of four types of Hydroxyapatite(HA)on CP Ti screws (micro HA, nano HA, dual nano HA with micro pores, dual nano HA with macro pores) where carbon particles used as fugitive material to be removed by thermal treatment to create porosity.For examination of the changes occurred on the substrate, SEM, SPM and XRD used, coatings characterized by XRD, SEM and interfacial shear strength measurements. Results:The results mentioned the formation of rutilenano TiO2 with, SEM showed that the size of pores in HA coatings corresponded to the size of carbon particles. Statistical analysis of the removal torque tests showed highest means of the single nano HA coating at 2 and 4 weeks implantation intervals. Histological analysisrevealed a faster reaction of bone and higher osteoblasts activity towards thermally oxidized CP Ti implants coated with single nano HA coating. Conclusion:Carbon particles as a fugitive material within nano HA coat produced porosity.Presence of pores ˃ 1µ in nano HA coats did not achieve highest removal torque values nor highest osteoblasts activity in 2 and 4 weeks implantation intervals. Keywords:Titanium, Thermal oxidization, Nano Hydroxyapatite, Coatings, porosity.
Background: Dental implants act as infrastructure for fixed restoration to look like as a natural tooth. Osseointegration is a biological events and considered as a base for success of dental implant. The aim of this study is to evaluate the bond strength between bone and Ti implant coated with mixture of nano hydroxyapatite-chitosan-collagen compared with Ti implants coated with nano hydroxyapatite implanted in rabbit tibia, after different period of implantation time (two and six weeks) by torque removal test. Material and methods: 36 screws of commercially pure titanium; 8mm in length and 3mm diameter , 18 screws coated with mixture of nano hydroxyapatite-chitosan-collagen and18 screws coated with nano hydroxyapatite by dip coating. St
... Show MoreBackground: The type of dental implant surface is one of many factors that determine the success of implant restoration. This study aimed to study the effect of mixture of nano titanium oxide with nanohydroxyapatite coating of screw shaped CPTi dental implant on bond strength at bone implant interface by torque removal test related to two healing periods (2 and 6 weeks). Materials and methods: Dip coating process was performed to get an even coating layer on CPTi screws. X-ray diffraction (XRD) analysis and microscopical examination were performed on the coating surfaces of the CPTi. The tibia of 10 white New Zealand rabbits was chosen as implantation sites. The tibia of each rabbit received two screws, one was coated with mixture of nanoT
... Show MoreBackground: Dental implant considers a unique treatment option for the replacement of missing dentition. The new trend of implants is looking for materials which accelerate bone formation in bone implant interface and enhance osseointegration to provide immediate loading directly after placement and decrease the time period which is disturbs patients and uncomfortable. The aim of the study was to evaluate the effect of nano zirconium oxide (ZrO2) and nano hydroxyapatite (Hap) mixture coating of screw shaped commercially pure titanium (cpTi) implants on bond strength at the bone implant interface with torque removal test and histological analysis in comparison with non coated implants. Materials and methods: Forty screws were machined from c
... Show MoreBackground: In recent years, the immediate loading of dental implants has become more accepted as a standard protocol for the treatment of the edentulous area. Success in implant dentistry depends on several parameters that may improve phenomenon of osseointegration and new bone formation in close contact with the implant. The aim of study was to evaluate the effect of strontium chloride coating of screw shape commercially pure titanium dental implant osseointegration at bone - implant interface by histomorphometric analysis and compare with hydroxyapatite coating at 2 time periods (2 weeks and 6 weeks). Materials and methods: Electrophoretic Deposition Technique (EPD) was used to obtain a uniform coating layer on commercially pure titanium
... Show MoreBackground: Dental implant surface technologies have been evolving rapidly to enhance a more rapid bone formation on their surface and improve implant therapy.Implant threads should be designed to increase surface contact areathat induced better stability. In addition, implant surface coating with Flaxseed was used to enhance bone formation at the bone-implant interface. Materials and methods: Ninety-six commercially pure titanium (CpTi) screws were implanted in rabbits' tibiae and divided into three groups as dual-threaded group, flaxseed-coated group and control group. All groups were evaluated mechanically, histologically and radiographically after each healing periods (2, 4, 6 and 8) weeks and the resulting data were statistically analy
... Show MoreBackground The application of nanotechnology to biomedical surfaces is explained by the ability of cells to interact with nanometric features. The aim of this study was to consider the role of nanoscale topographic modification of CPTi dental implant using chemical etching method for the purpose of improving osseointegration. Materials and methods: Commercial pure titanium rod was machined into 20 dental implants. Each implant was machined in diameter about 3mm, length of 8mm (5mm was threaded part and 3mm was flat part). Implants were prepared and divided into 2 groups according to the types of surface modification method used: 1st group (10 implant) remained without nano surface modification (control), 2nd group include (10 implant) etche
... Show MoreIn this research we investigated the corrosion behavior of the commertialy pure titanium and Ti-6Al-4V alloy that coated with hydroxyapatite by electrochemical deposition with applied voltage (6,9,12) Volt from aqueous solution containing Ca(NO3)2.H2O =7.0 gm/l , (NH4)2HPO4 =3.5 gm/l , Na(NO3)2 = 8.5 gm/l in order to improve the bonding strength of hydroxyapetite and medical metals and alloys and increasing the biocompatibility. The coating layer morphology was investigated by XRD, Optical microscope , and SEM tests, the corrosio tests was made by use senthesys simulated body fluid (SBF) , and we found that the propreate voltage for coatint on Ti was 9 Volt and for Ti-6Al-4Vwas12Volt.
In this study, a Hydroxyapatite (HA) coating was prepared on a titanium implant by an electrochemical deposition process. The titanium pre-treatment by anodizing in 1.65 mol/L sulfuric acid with (10V) at room temperature. The deposition was all conducted at a constant voltage of 6.0 V, for 1 h at room temperature. The coatings thus prepared were characterized with Fourier transform infrared spectroscopy (FTIR) and thickness of the coated layer.The electrochemical deposition of HA occurred on the titanium as a cathode. Coated titanium by HA after anodizing revealed a good corrosion protection efficiency even at a temperature ranged (293-323) K in artificial saliva. Activation energy and pre-exponential factor (kinetic parameters) were calcul
... Show MoreObjective This study evaluated the effects of adding titanium oxide (TiO2) nanofillers on the tear strength, tensile strength, elongation percentage, and hardness of room-temperature-vulcanized (RTV) VST50F and high-temperature-vulcanized (HTV) Cosmesil M511 maxillofacial silicone elastomers. Methods Two types of maxillofacial elastomers, VST50F RTV and Cosmesil M511 HTV, were used. Nano-TiO2 powder was applied as a nanofiller. A total of 120 specimens were fabricated, 60 each of VST50F and Cosmesil M511. The specimens of each type of elastomer were divided into three equal groups on which tests were conducted for tear strength, tensile strength, and hardness i.e., 20 specimens were used for each test. Each group of 20 specimens was further
... Show More