PVA, Starch/PVA, and Starch/PVA/sugar samples of different
concentrations (10, 20, 30 and 40 % wt/wt) were prepared by casting
method. DSC analysis was carried; the results showed only one glass
transition temperature (Tg) for the samples involved, which suggest
that starch/PVA and starch/PVA/sugar blends are miscible. The
miscibility is attributed to the hydrogen bonds between PVA and
starch. This is in a good agreement with (FTIR) results. Tg and Tm
decrease with starch and sugar content compared with that for
(PVA). Systematic decrease in ultimate strength, due to starch and
sugar ratio increase, is attributed to (PVA), which has more hydroxyl
groups that made its ultimate strength higher than that for
starch/PVA, and starch/PVA/sugar blends. It is observed from water
uptake tests that the solubility time decreases with starch ratio; it is
attributed to decrease in hydroxyl groups caused by PVA ratio
decrease. The inter- and inter-molecular bonds of the hydroxyl
groups enhanced the solubility process of the starch/PVA blends in
water. The water immersion causes hydrogen bonds (inter and
intermolecular bonds) to decompose, that increases the film
solubility. Water absorption and capacity of degradability are most
important in biodegradable materials. The results suggest the samples
that have undergone investigation, can be used for shopping, and
food packaging.
The study of soil burial for the sample at (3cm) depth, and at (13cm)
depth has exhibited weight loss increase with soil burial time. The
biodegradability rapidly increases at the first (6-7) weeks; it is found
that the weight loss at (3cm) depth is greater than that at (13cm) that
was attributed to the differences in the availability of oxygen ratio. It
is found that PVA undergoes lowest weight loss, the weight loss
changes with starch, and sugar content. In dry soil, the weight loss is
lower. The results proved that the biodegradation decreases with soil
burial time after seven weeks of burial. It is concluded that the
samples involved are biodegradable material that can be used for
packaging applications and biologically friendly synthetic polymer
blends to solve the solid waste accumulation problem.
A simple and accurate method to determinate furosemide (FUR) based on converting the secondary amine to primary amine with acidic hydrolysis then azotization by nitrous acid and coupled with resorcinol as a coupling agent in aqueous medium at pH 13. The optical characteristic like beers law limit found to be (0.25-2.5) μg.ml−1, detection and quantification limits (0.0196) (0.0654) μg.ml−1respectivly and Sandel sensitivity was 0.006738 μg.cm−2. The least-square method was used to evaluate the regression equation and the correlation coefficient. The resulted azo dye has a maximum absorbance at 430 nm with light oran
This research is marked by " lighting and processors formalism for spaces of shops selling mobile phones ," aims to " reveal about the relationship between lighting treatments formal designs spaces own internal selling mobile phone in addition to the recognition criteria Altsamama to lighting techniques and processes formality spaces shops competent to sell mobile phone " and lies the importance of this research in the " active role of the lighting in the building processors formalities and processes to prepare designs and show the final form integrated functionally and aesthetically so as to be ready for implementation , taking into consideration the role expressionist in the recipient and to make these spaces more than meet the require
... Show MoreA new method for determination of allopurinol in microgram level depending on its ability to reduce the yellow absorption spectrum of (I-3) at maximum wavelength ( ?max 350nm) . The optimum conditions such as "concentration of reactant materials , time of sitting and order of addition were studied to get a high sensitivity ( ? = 27229 l.mole-1.cm-1) sandal sensitivity : 0.0053 µg cm-2 ,with wide range of calibration curve ( 1 – 9 µg.ml-1 ) good stability (more then24 hr.) and repeatability ( RSD % : 2.1 -2.6 % ) , the Recovery % : ( 98.17 – 100.5 % ) , the Erel % ( 0.50 -1.83 % ) and the interference's of Xanthine , Cystein , Creatinine , Urea and the Glucose in 20 , 40 , 60 fold of analyate were also studied .
The present research was conducted to synthesis Y-Zeolite by sol-gel technique using MWCNT (multiwalled carbon nanotubes) as crystallization medium to get a narrow range of particle size distribution with small average size compared with ordinary methods. The phase pattern, chemical structure, particle size, and surface area were detected by XRD, FTIR, BET and AFM, respectively. Results shown that the average size of Zeolite with and without using MWCNT were (92.39) nm and (55.17) nm respectively .Particle size range reduced from (150-55) nm to (130-30) nm. The surface area enhanced to be (558) m2/g with slightly large pore volume (0.231) km3/g was obtained. Meanwhile, degree of crystallization decrease
... Show MoreABSTRACT : Fifteenth isolates of C. sakazakii were obtained from previous studies of the sample (infant formula, cerebrospinal fluid and blood). All isolates C. sakazakii identification based on microscopic, biochemical test and confirmed by 16SrRNA. We studied the movement of all isolates and study adhesion to polystyrene plate, adhesion and invasion to Esophageal adenocarcinoma (SKG-GT-4) for four isolates [Cerebrospinal fluid (CSF5), Bloods (B 1), Dialak (A1c), Novolac Allernova (C1)] and its cytotoxicity. Results showed that all isolates can move after 4 hours of incubation and increased after 8 hours, the isolates moved to different distances strong, medium, and weak. The results showed that the number of C. sakazakii colony adherent t
... Show More