The influence of sintering and annealing temperatures on the structural, surface morphology, and optical properties of Ag2Cu2O4 thin films which deposited on glass substrates by pulsed laser deposition method have been studied. Ag2Cu2O4 powders have polycrystalline structure, and the Ag2Cu2O4 phase was appear as low intensity peak at 35.57o which correspond the reflection from (110) plane. Scan electron microscopy images of Ag2Cu2O4 powder has been showed agglomerate of oxide particles with platelets shape. The structure of thin films has been improved with annealing temperature. Atomic Force micrographs of Ag2Cu2O4 films showed uniform, homogenous films and the shape of grains was almost spherical and larger grain size of 97.85 nm has obtained for film sintered at 600 °C. The optical band gap was increase from 1.6 eV to 1.65 eV when sintering temperature increased to 300 °C and decrease to 1.45 eV at 600 °C for the films deposited at room temperature. Heat treatment of films has been increased the energy band with increasing sintering temperature. Hall coefficient of Ag2Cu2O4 films have a positive sign which means the charge carrier is a p-type. The electrical conductivity decreases with increasing of the sintering temperature for as deposited and annealed films.
The effect of annealing on the structural and optical properties of Antimony trisulfide (Sb2S3) is investigated. Sb2S3 powder is vaporized on clean glass substrates at room temperature under high vacuum pressure to form thin films. The structural research was done with the aid of X-ray diffraction (XRD) and atomic force microscopy (AFM). The amorphous to the polycrystalline transformation of these thin films was shown by X-ray diffraction analysis after thermal annealing. These films' morphology is explained. The absorption coefficient and optical energy gap of the investigated films are calculated using transmission spectra. Both samples have strong absorption in the visible spectrum, according to UV-visible absorption spectra. The optical
... Show MoreCadmium Oxide and Bi doped Cadmium Oxide thin films are prepared by using the chemical spray pyrolysis technique a glass substrate at a temperature of (400?C) with volumetric concentration (2,4)%. The thickness of all prepared films is about (400±20) nm. Transmittance and Absorbance spectra are recorded in the wave length ranged (400-800) nm. The nature of electronic transitions is determined, it is found out that these films have directly allowed transition with an optical energy gap of (2.37( eV for CdO and ) 2.59, 2.62) eV for (2% ,4%) Bi doped CdO respectively. The optical constants have been evaluated before and after doping.
Chalcopyrite thin films were one-step potentiostatically deposited onto stainless steel plates from aqueous solution containing CuSO4, In2(SO4)3 and Na2S2O3.The ratio of (In3+:Cu2+) which involved in the solution and The effect of cathodic potentials on the structural had been studied. X-ray diffraction (XRD) patterns for deposited films showed that the suitable ratio of (In3+:Cu2+) =6:1, and suitable voltage is -0.90 V versus (Ag/AgCl) reference electrode
Thin films of CdS:Cu were deposited onto glass substrate temperature 400 °c. The optieal properties have been studied for Cds doped with (1,3, 8) wt% of Cu before and after Gamma irradiation. It was found that the irradiation caused an ( Frenkel defects) where the atom is displaced from its original site leaving vacancy and forming on interstitial atom. It was found the irradiation caused an absorption edge shifting towards long wavelength as a result of the increasing of Cu concentration.
This paper presents the effect of Cr doping on the optical and structural properties of TiO2 films synthesized by sol-gel and deposited by the dip- coating technique. The characteristics of pure and Cr-doped TiO2 were studied by absorption and X-ray diffraction measurement. The spectrum of UV absorption of TiO2 chromium concentrations indicates a red shift; therefore, the energy gap decreases with increased doping. The minimum value of energy gap (2.5 eV) is found at concentration of 4 %. XRD measurements show that the anatase phase is shown for all thin films. Surface morphology measurement by atomic force microscope (AFM) showed that the roughness of thin films decrease with doping and has a minimum value with 4 wt % doping ratio.
Compounds from ZnO doped with AgO in different ratio (0,3,5,7, and 9)wt.% were prepared.Thin films from the prepared compounds were deposited on a glass substrate using the pulsed laser deposition method. The XRD pattern confirmed the presence of a single-phase hexagonal wurtzite ZnO structure, without the presence of a secondary phase. AFM measurements showed an increase in both average grain size and average surface roughness with increasing concentration content of (AgO).The crystallite size of ZnO of the main peak corresponding to the preferred plane of crystal growth named (100) increases from 17.8 to 22.5nm by increasing of AgO doping ratio from 0 to 9%. The absorbance and transmittance in the wavelength range (350-1100 nm) were
... Show MoreIn this Research, (In2O3: CdO) films were prepared using pulsed laser deposition (PLD) method on glass substrate at room temperature deposited at laser influence 500mJ/cm2with different shoots N= (200,300,400,500and600). the structural, and the optical properties and the films are studied with different annealing temperatures (523and 623) K. Optical measurements and the films were analyzed by UV-VIS absorption spectra. The structural properties of samples were investigated by x-ray diffraction patterns of the films and show that the films and polycrystalline Structure with all shoots. Transmittance spectrum found is equal to 93.17%, refractive index range is 1.635 and energy gap range is 2.75-3.15ev.
In this research the Cobalt Oxide (Co3O4) films are prepared by the method of chemical spray pyrolysis deposition at different thicknesses such that (250, 350, 450, and 550) ± 20 nm. The optical measurement shows that the Co3O4 films have a direct energy gap, and they in general increase with the increase of the thickness. The optical constants are investigated and calculated such as absorption coefficient, refractive index, extinction coefficient and the dielectric constants for the wavelengths in the range (300-900) nm. The electrical conductivity (σ) and the activation energies (Ea1, Ea2) have been investigated on (Co3O4) thin films as a function of thickness. The films
... Show MoreIn the present work we prepared heterojunction not homogenous CdS/:In/Cu2S) by spray and displacement methods on glass substrate , CdS:In films prepared by different impurities constration. Cu2S prepared by chemical displacement method to improve the junction properties , structural and optical properties of the deposited films was achieved . The study shows that the film polycrystalline by XRD result for all film and the energy gap was direct to 2.38 eV with no effect on this value by impurities at this constration .