This work is concerned with the synthesis of two types of composites thin films (Sb2O3:WO3 and (Sb2O3:In2O3) with different concentrations (0.0,0.05,0.1, and 0.15). The prepared thin films are characterized with the use of the X-ray diffraction atomic force microscope AFM and UV-Vis–infrared spectrophotometer. The structural examination shows that both composite's thin films were polycrystalline with nano size with cubic phase as majority and orthorhombic phase as minority phase. The crystal size decreases from 34.6 to 24.7 and 21.7 nm for (Sb2O3:WO3) and (Sb2O3:In2O3) thin films, respectively. The average roughness shows non-regular growth by increasing the concentration of both oxides. The optical energy band gap shows a red shift for both types of nanostructure thin films, which populate these composited thin films for solar cell applications.
The optical energy gap(Eopt) and the width of the tails of localized states in the band gap (?E) for Se:2%Sb thin films prepared by thermal co-evaporation method as a function of annealing temperature are studied in the photon energy range ( 1 to 5.4)eV.Se2%Sb film was found to be indirect transition with energy gap of (1.973,2.077, 2.096, 2.17) eV at annealing temperature (295,370,445,520)K respectively. The Eopt and ?E of Se:2%Sb films as a function of annealing temperature showed an increase in Eopt and a decrease in ?E with increasing the annealing temperature. This behavior may be related to structural defects and dangling bonds.
(Cu1-x,Agx)2ZnSnSe4 alloys have been fabricated with different Ag content(x=0, 0.1, and 0.2) successfully from their elements. Thin films of these alloys have been deposited on coring glass substrate at room temperature by thermal evaporation technique under vacuum of 10-5Torr with thickness of 800nm and deposition rate of 0.53 nm/sec. Later, films have been annealed in vacuum at (373, and 473)K, for one hour. The crystal structure of fabricated alloys and as deposited thin films had been examined by XRD analysis, which confirms the formation of tetragonal phase in [112] direction, and no secondary phases are founded. The shifting of main polycrystalline peak (112) to lower Bragg’s angle as compared to Cu2ZnSnSe4 angle refers to incorpora
... Show MoreThe effect of different doping ratio (0.3, 0.5, and 0.7) with thickness in the range 300nmand annealed at different temp.(Ta=RT, 473, 573, 673) K on the electrical conductivity and hall effect measurements of AgInTe2thin film have and been investigated AgAlxIn(1-x) Te2 (AAIT) at RT, using thermal evaporation technique all the films were prepared on glass substrates from the alloy of the compound. Electrical conductivity (σ), the activation energies (Ea1, Ea2), Hall mobility and the carrier concentration are investigated as a function of doping. All films consist of two types of transport mechanisms for free carriers. The activation energy (Ea) decreased whereas electrical conductivity increases with increased doping. Results of Hall Effect
... Show MoreThe electrical properties of polycrystalline cadmium telluride thin films of different thickness (200,300,400)nm deposited by thermal evaporation onto glass substrates at room temperature and treated at different annealing temperature (373, 423, 473) K are reported. Conductivity measurements have been showed that the conductivity increases from 5.69X10-5 to 0.0011, 0.0001 (?.cm)-1 when the film thickness and annealing temperature increase respectively. This increasing in ?d.c due to increasing the carrier concentration which result from the excess free Te in these films.
ZnO thin films have been prepared by pulse laser deposition technique at room temperatures (RT). These films were deposited on GaAs substrate to form the ZnO/GaAs heterojunction solar cell. The effect of annealing temperatures at ( RT,100, 200)K on structural and optical properties of ZnO thin films has been investigated. The X-ray diffraction analysis indicated that all films have hexagonal polycrystalline structure. AFM shows that the grains uniformly distributed with homogeneous structure. The optical absorption spectra showed that all films have direct energy gap. The band gap energy of these films decreased with increasing annealing temperatures. From the electrical properties, the carriers have n-type conductivity. From
... Show MorePulsed laser deposition (PLD) technique was applied to prepared Chromium oxide (Cr2O3) nanostructure doped with Titanium oxide (TiO2) thin films at different concentration ratios 3,5,7 and 9 wt % of TiO2. The effect of TiO2 dopant on the average size of crystallite of the synthesized nanostructures was examined by X-ray diffraction. The morphological properties were discussed using atomic force microscopy(AFM). Observed optical band gap value ranged from 2.68 eV to 2.55 eV by ultraviolet visible(UV-Vis.) absorption spectroscopy with longer wave length shifted in comparison with that of the bulk Cr2O3 ~3eV. This indicated that the synthesized samples a
... Show MoreThis study investigates the influence of silver oxide (Ag₂O) nanoparticles on the gas-sensing properties of carbon nanotube (CNT) and poly(3-hexylthiophene) (P3HT) composite films. The goal is to enhance the sensitivity and stability of CNT/P3HT-based gas sensors for nitrogen dioxide (NO₂) detection. CNTs and P3HT are composited at various mass ratios, followed by integrating Ag₂O nanoparticles to improve gas interaction and electronic properties. Structural and morphological analyses, including x-ray diffraction, Fourier transform infrared spectroscopy, field emission scanning electron microscopy, and energy dispersive x-ray spectroscopy, ascertain the successful incorporation of Ag₂O into the composites and reveal its role in impr
... Show Morein this paper copper oxide (cuO thin films were prepared by the method of vacum thermal evaporation a pressure.