Background: Denture lining materials are widely used in prosthodontic treatment and management of traumatized oral mucosa. A contaminated prosthesis can provide a source of cross-contamination between patients and dental personnel as well as a cause for denture stomatitis. Therefore, denture disinfection has been recommended as an essential procedure for maintenance of a healthy oral mucosa. This study investigated the effect of SOLO disinfectant solution on some properties of different denture lining materials. Materials and methods: Three different solutions were used in this study; SOLO disinfectant solution, sodium hypochlorite solution, and water on three types of acrylic denture lining materials; hot cure, cold cure, and soft acrylic resin. Twenty seven disk-shaped samples were used to evaluate the color stability and forty five rectangular samples were used for testing the surface micro hardness and surface roughness of the different denture lining materials. Data measurements of the color stability, surface hardness, and surface roughness were analyzed and compared statistically. Results: The color stability for the tested denture lining materials was insignificantly affected (p>0.05) by the immersion in the SOLO disinfectant solution. There was a highly significant difference (p< 0.01) in the surface hardness of the hot cure while it was insignificant (p>0.05) for cold cure denture lining materials when immersed in the SOLO disinfectant solution. For surface roughness there was no significant difference (p>0.05) by immersion in SOLO disinfectant solution for the different denture lining materials. Conclusions: Based on the results of this study SOLO disinfectant solution produced no adverse effect on the color stability, surface hardness, and surface roughness of the hot cure, cold cure, and soft acrylic denture lining materials
Background: The geriatric patients wearing removable partial dentures are increasing in proportion. At the same time, the root caries prevalence accompanied by gingival recession is increasing. A variety of vehicles can deliver fluoride into the oral cavity, including fluoride mouth-rinse, fluoride dentifrice, topical fluoride, and fluoride-releasing restorative materials, all of which effectively prevent root caries and suppress recurrent caries. This study aimed to evaluate the effect of sodium fluoride addition on some mechanical properties of heat cure acrylic denture base material. Material and method: A total of 90 samples were prepared in this study, then divided into three main groups according to the type of test used (hardness, te
... Show MoreIn this research, the effect of adding two different types of reinforcing particles was investigated, which included: nano-zirconia (nano-ZrO2) particles and micro-lignin particles that were added with different volume fractions of 0.5%, 1%, 1.5% and 2% on the mechanical properties of polymer composite materials. They were prepared in this research, as a complete prosthesis and partial denture base materials was prepared, by using cold cure poly methyl methacrylate (PMMA) resin matrix. The composite specimens in this research consist of two groups according to the types of reinforced particles, were prepared by using casting methods, type (Hand Lay-Up) method. The first group consists of PMMA resin reinforced by (nano-ZrO
... Show MoreBackground: In dentistry, dentist takes the advantages of soft lining materials due to the viscoelastic properties. The major problem is the adhesion of the soft liner with the denture base material. Materials and Methods: Heat cured of high impact acrylic resin specimens prepared with dimensions 75x13x13mm for shear bond strength test, soft lining material (Refit and Mollosil) with a 3-mm thickness and used to join each two acrylic blocks. Also four specimens with the same previous dimensions utilized for chemical and physical surface analysis. The specimens grouped as control (without plasma) and experiment (with oxygen plasma) treated high impact acrylic specimens. Results: Plasma treatment increased the shear bond strength for both Refi
... Show MoreBackground: Impression materials, impression trays, and poured stone cast have been said to be the main source of cross infection between patients and dentists. However, it was observed that disinfection of the impression is not performed systematically in routine dental practice. Disinfection of alginates either by immersion or spray technique was found to cause dimensional inaccuracies, although with proper disinfection of alginates there were small dimensional changes. A variety of fluoride releasing products designed for topical use is currently available. Following their use, varied amount of fluoride is systemically absorbed depending on the fluoride concentration and the manner of its use. The objective of this study was to evaluate
... Show MoreBackground: Polymethylmethacrylate (PMMA) has relatively unsatisfactory mechanical properties such as low flexural strength and impact strength also dimensional instability. Material and method: Zirconium silicate nanoparticles were coated with a layer of trimethoxysilylpropylmethacrylate (TMSPM) before sonication in monomer (MMA) with the percentages 1% and 1.5% by weight then mixed with powder using conventional procedure, (150) samples were prepared and divided into three groups, each group consisted of (50) samples, the first group prepared from PMMA without addition (control), another group with the addition of 1% wt Zrsio4 nanoparticles (experimental) and the third one with 1.5% wt Zrsio4 nanoparticles (experimental). Each group
... Show MoreBackground: Fracture of different types of acrylic denture base is a common problem associated with dental prosthesis. Studies suggested that the repair strength may be improved by several means including surface treatment with chemical agents. The aim of the study was to evaluate the effect of surface treatment with acrybond-bonding agent and monomer on fractured denture base in respect to transverse, tensile and shear bond strength and evaluation of the mode of failure by light microscope. Materials and methods: Two hundred seventy specimens were prepared and divided into 3 groups according to the material used (regular conventional, rapid simplified and high impact) heat cure acrylic. The specimen in each groups were prepared specificall
... Show MoreAims: This study was conducted to assess the effect of the addition of yttrium oxide (Y2O3) nanoparticles on the tensile bond strength, tear strength, shore A hardness, and surface roughness of soft-denture lining material. Materials and Methods: Y2O3 NPs with 1.5 and 2 wt.% were added into acrylic-based heat-cured soft-denture liner. A total of 120 specimens were prepared and divided into four groups according to the test to be performed (tensile bond strength, tear strength, surface hardness, and surface roughness). Results: There was a highly significant increase in tensile bond strength between the soft liner and the acrylic denture base, tear strength, and hardness at both concentrations as compared to the control group, whereas ther
... Show MoreBackground: Polymethyl methacrylate (PMMA) is the most commonly used material in denture fabrication. The material is far from ideal in fulfilling the mechanical requirement. The purpose of this study was to evaluate the effect of addition of 3% wt of treated (silanized) Titanium oxide Nano filler on some physical and mechanical properties of heat cured acrylic denture base material. Materials and methods: 100 specimens were constructed, 50 specimens were prepared from heat cure PMMA without additives (control) and 50 specimens were prepared from heat cure PMMA with the addition of TiO2 Nano fillers. Each group was divided into 5 sub groups according to the test performed which was mixed by probe ultra-sonication machine. Results: A highly
... Show MorePolymer matrix composites are suitable materials for medical applications, such as denture base resin polymethyl methacrylate (PMMA). This includes light weight and high strength. This paper describes the effect of selected weight fractions (1, 2, 3, 4 & 5) % wt of nano(Alumina AL2O3, Zirconia ZrO2, Hydroxyapatite HA and Halloysite nanoClay) reinforcements on the biopolymer matrix (PMMA). Some tribology tests were used to evaluate the prepared system (impact strength, hardness surface, and wear rate) tests. The samples were fabricated by (Hand Lay-Up) with different particle reinforcement percentages. All tests were accomplished at room temperature, and samples were developed according to the ASTM standard. The weight fraction o
... Show More