Bulk AlxSb1-x samples were prepared with different x ratios (0.1, 0.3, 0.5, 0.7 and 0.9) by quenching technique. This was done throughout mixing the aluminum and antimony elements according to the proper atomic weight and put them in an evacuated quartz ampoule which then sealed and heated at 1273 K for five hours and left to cool in air. Thin films of AlxSb1-xwere prepared by using thermal evaporation under vacuum of 10-5 mbar on glass substrates at room temperature with deposition rate (10-15nm/min) at thickness of ∼ 500nm. The structures of AlxSb1-x bulk and thin films have been studied by X–ray diffraction technique. The results showed that all alloys have polycrystalline structures and the peaks at composition ratio x = 0.3, 0.5 and 0.7 were identical with the AlSb standard peaks while at x = 0.1 and 0.9 the peaks are identical with Sb and Al respectively. The x-ray pattern of the prepared thin films are polycrystalline and the peaks identical with cubic structure also the peaks intensity decrease with the increase of aluminum ratio in the prepared thin films. AFM measurements showed the non-regular variation (increasing and decreasing) of both the average grain size and average surface roughness with the increasing of composition ratio. AlxSb1-x thin films showed high charge carrier concentration nHespecially at x = 0.1 and 0.3 on the other side charge carrier concentration showed reduction with the increase of aluminum content whereas nHreach minimum value at x = 0.7 and then increases with further increase of aluminum content. The electrical conductivity of AlxSb1-x declare similar behavior where it reach minimum value at x = 0.5. From another side AlxSb1-x thin films show high conductivity resemble that of metallic material especially also at x = 0.1 and 0.3.
Chalcogenide glasses SeTe have been prepared from the high purity constituent elements .Thin films of SeTe compound have been deposited by thermal evaporation onto glass substrates for different values of film thickness . The effect of varying thickness on the value of the optical gap is reported . The resultant films were in amorphous nature . The transmittance spectra was measured for that films in the wavelength range (400-1100) nm . The energy gap for such films was determined .
Indium Antimonide (InSb) thin films were grown onto well cleaned glass substrates at substrate temperatures (473 K) by flash evaporation. X-ray diffraction studies confirm the polycrystalline of the films and the films show preferential orientation along the (111) plane .The particle size increases with the increase of annealing time .The transmission spectra of prepared samples were found to be in the range (400-5000 cm-1 ) from FTIR study . This indicates that the crystallinity is improved in the films deposited at higher annealing time.
Radiation is a form of energy, its emitted either in the form of particles such as α-particles and β-particles (beta particles including the electron and the positron) or waves such as sunlight, X-rays and γ-rays. Radiation found everywhere around us and it comes from many different sources naturally or man-made sources. In this study a questionnaire was distributed to people working in the field of X-rays that used for a medical imaging (X-ray and CT-scan) to evaluate the extent of awareness and knowledge in estimate the damage of ionizing radiation as a result of wrong use. The questionnaire was distributed to medical clinics in Al-Harithiya in Baghdad, which it’s considered as
Abstract: This paper presents the results of the structural and optical analysis of CdS thin films prepared by Spray of Pyrolysis (SP) technique. The deposited CdS films were characterized using spectrophotometer and the effect of Sulfide on the structural properties of the films was investigated through the analysis of X-ray diffraction pattern (XRD). The growth of crystal became stronger and more oriented as seen in the X-ray diffraction pattern. The studying of X-ray diffraction showed that; all the films have the hexagonal structure with lattice constants a=b=4.1358 and c=6.7156A°, the crystallite size of the CdS thin films increases and strain (ε) as well as the dislocation density (δ) decreases. Also, the optical properties of the
... Show MoreDuring of Experimental result of this work , we found that the change of electrical conductivity proprieties of tin dioxide with the change of gas concentration at temperatures 260oC and 360oC after treatment by photons rays have similar character after treatment isothermally. We found that intensive short duration impulse annealing during the fractions of a second leads to crystallization of the films and to the high values of its gas sensitivity.
ZnIn2(Se1-xTex)4 (ZIST) chalcopyrite semiconductor thin films at various contents (x = 0.0, 0.2, and 0.4) are deposited on glass and p type silicon (111) substrate to produce heterojunction solar cell by using the thermal evaporation technique at RT where the thickness of 500 nm with a vacuum of 1×10-5 mbar and a deposited rates of 5.1 nm/s. This study focuses on how differing x content effect on the factors affecting the solar cell characteristics of ZIST thin film and n-ZIST/p-Si heterojunction. X-ray diffraction XRD investigation shows that this structure of ZIST film is polycrystalline and tetragonal, with (112) preferred orientation at 2θ ≈ 27.01. Moreover, atomic force microscopy AFM is studying the external morphology of
... Show More