The disposal of the waste material is the main goal of this investigation by transformation to high-fineness powder and producing self-consolidation concrete (SCC) with less cost and more eco-friendly by reducing the cement weight, taking into consideration the fresh and strength properties. The reference mix design was prepared by adopting the European guide. Five waste materials (clay brick, ceramic, granite tiles, marble tiles, and thermostone blocks) were converted to high-fine particle size distribution and then used as 5, 10, and 15% weight replacements of cement. The improvement in strength properties is more significant when using clay bricks compared to other activated waste ceramics and granite tiles. The percentage increases to 11.59% at 28 days for compressive strength when using 10% replacement of cement weight. The ability to produce eco-SCC with less cement content and lower cost consumption is encouraged, although the enhancement in strength is not high since the waste can be disposable. While the percentage reduction in the strength of SCC mixes containing marble tile or thermostone block powder increases with the replacement of cement weight with a greater need for superplasticizer justification, we recommend using 5% as a replacement by weight of cement with an insignificant retardation of strength. Finally, there is a good relationship between compressive strength and ultrasonic pulse velocity and between tensile and flexural strength with a high
Worldwide, enormous amounts of waste cause major environmental issues, including scrap tires and plastic, and large waste, a consequence of the demolition of buildings, including crushed concrete, crushed clay bricks, and crushed thermo-stone. From that point, it’s possible to consider that the recycling processes for these materials and using them in the manufacturing field will reduce the adverse effects on the environment of these wastes and the consumption of natural resources. Sustainable concrete blocks can be considered as one of the products produced by using these materials as partial volume replacement of the coarse, fine aggregate, or cement content, considering their dry density, workability, absorption, compressive st
... Show MoreThis research of using Feldspar in the production self compacting concrete (SCC) ( 5,10,15 )% as partial replacement by weight of cement .In this research some of fresh properties of SCC ( slump flow used V-funnel test and filling ability used ( U- box test ) for concrete mixes and also some of the harden properties of SCC ( compressive and flexural tests ). The research results showed that negative effect of Feldspar on the fresh properties of self compacting concrete but the positive effect of Feldspar on the harden properties of self compacting concrete .
Waste materials might be utilized in various applications, such as sustainable roller compacted concrete pavements (RCCP), to lessen the negative environmental consequences of construction waste. The impacts of utilizing (brick, thermostone, granite, and ceramic) powders on the mechanical characteristics of RCCP are investigated in this study. To achieve this, the waste materials were crushed, grounded, and blended before being utilized as filler in the RCCP. After the mixes were prepared, compressive strength, splitting tensile strength, flexural strength, water absorption, density, and porosity were all determined. According to the research results, adding some of these powders, mainly brick and granite powder, enhances the mechanical
... Show MoreThis article investigates the development of the following material properties of concrete with time: compressive strength, tensile strength, modulus of elasticity, and fracture energy. These properties were determined at seven different hydration ages (18 h, 30 h, 48 h, 72 h, 7 days, 14 days, 28 days) for four pure cement concrete mixes totaling 336 specimens tested throughout the study. Experimental data obtained were used to assess the relationship of the above properties with the concrete compressive strength and how these relationships are affected with age. Further, this study investigates prediction models available in literature and recommendations are made for models that are found suitable for application to early age conc
... Show MoreAbstract
The current research sought to demonstrate the effect of material flow cost accounting on reducing products through the application of material flow cost accounting technique, which works on the optimal utilization of materials and energy and the reduction of environmental impacts.The research aims to clarify the knowledge foundations for material flow cost accounting, in addition to studying the material flow cost accounting technique that helps reduce the cost of products and make them environmentally friendly. To achieve this, the research relied on the descriptive approach with regard to the theoretical aspect of the resea
... Show MoreMost of the recent works related to the construction industry in Iraq are focused on investigating the validity of local raw materials as alternatives to the imported materials necessary for some practical applications, especially in thermal and sound insulation. This investigation includes the use of limestone dust as partial substitution of cement in combination with foam agent and silica fume to produce sustainable Lightweight Foam Concrete (LWFC). This study consists of two stages. In the first stage, trial mixes were performed to find the optimum dosage of foam agent. Limestone dust was used as a partial replacement for cement. Chemical analysis and fineness showed great similarity with cement. Many concrete mixes were prepared
... Show MoreThe massive growth of the automotive industry and the development of vehicles use lead to produce a huge amount of waste tire rubber. Rubber tires are non-biodegradable, resulting in environmental problems such as fire risks. In this search, the flexural behavior of steel fiber reinforced self-compacting concrete (SFRSCC) beams containing different percentages and sizes of waste tire rubbers were studied and compared them with the flexural behavior of SCC and SFRSCC. Micro steel fiber (straight type) with aspect ratio 65 was used in mixes. The replacement of coarse and fine aggregate was 20% and 10% with chip and crumb rubber. Also, the replacement of limestone dust and silica fume was 50%, 25%, and 12% with ground rubbe
... Show More