In this paper, the effect of sulfur substitution by arsenic on the structural, optical properties of thin films of the trivalent chalcogenide Se66S44-xAsx at different concentrations (where x = 0, 8, 16, and 24 at %) was studied. Thin films with a thickness of (300±10 nm) were prepared using thermal evaporation of bulk samples. Structural examinations were performed using XRD and AFM techniques. All the studied film samples were amorphous in structure and the intensity of the crystalline parts was high in the range of 10-40. Also, in Atomic Force Microscopy (AFM). It was found that increasing the concentration of arsenic affects the structural parameters such as surface roughness, particle density, and average grain size. As the arsenic element increased by 0.24, the grains became more regular, and the particle density increased. UV-Vis measurements reveal that the prepared films' absorption in the spectral wavelength range from 200 to 1100 nm. It was found that increasing the arsenic content led to a change in the absorbance of the films. The optical energy gap of Se66S44-xAsx thin films was determined and it was found that increasing arsenic content affected the energy gap differently as it changed within the range (2.35-2.19 eV). The energy gap increased at concentrations of (8, 16%) while the energy gap decreased at concentrations of 24%.
Au nanoparticle-functionalized (TiO2)1−x(ZnO:MgO)x nanocomposite thin films (0≤x≤0.3) were effectively produced by chemical spray pyrolysis and annealed at 600 °C. The effects of ZnO incorporation and Au nanoparticle modification on the films' structural, optical, and antibacterial properties were studied using X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FTIR), UV–Vis spectroscopy, and field-emission scanning electron microscopy (FESEM). XRD analysis confirms the formation of polycrystalline anatase TiO2 and shows a composition-dependent structural develop- ment with increasing ZnO concentration. The optical experiments revealed increased transmittance and a progressive wid- ening of the optical band gap f
... Show MoreA thin CdS Films have been evaporated by thermal evaporation technique with different thicknesses (500, 1000, 1500 and 2000Å) and different duration times of annealing (60, 120 180 minutes) under 573 K annealing temperature, the vacuum was about 8 × 10-5 mbar and substrate temperature was 423 K. The structural properties of the films have been studied by X- ray diffraction technique (XRD). The crystal growth became stronger and more oriented as the film thickness (T) and duration time of annealing ( Ta) increases.
The structural, optical and electrical properties of ZnS films prepared by vacuum evaporation technique on glass substrate at room temperature and treated at different annealing temperatures (323, 373, 423)K of thickness (0.5)µm have been studied. The structure of these films is determined by X-ray diffraction (XRD). The X-ray diffraction studies show that the structure is polycrystalline with cubic structure, and there are strong peaks at the direction (111). The optical properties investigated which include the absorbance and transmittance spectra, energy band gab, absorption coefficient, and other optical constants. The results showed that films have direct optical transition. The optical band gab was found to be in the range t
... Show MoreThe influence of the reaction gas composition during the DC magnetron sputtering process on the structural, chemical and optical properties of Ce-oxide thin films was investigated. X-ray diffraction (XRD) studies confirmed that all thin films exhibited a polycrystalline character with cubic fluorite structure for cerium dioxide. X-ray photoelectron spectroscopy (XPS) analyses revealed that cerium is present in two oxidation states, namely as CeO2 and Ce2O3, at the surface of the films prepared at oxygen/argon flow ratios between 0% and 7%, whereas the films are completely oxidized into CeO2 as the aforementioned ratio increases beyond 14%. Various optical parameters for the thin films (including an optical band gap in the range of 2.25–3.
... Show MoreIn this study the alloys Ge xS1-x with different Ge content (x=0, 0.1,0.2 and 0.3) wt.% have been successfully prepared by evacuated quartz tube under vacuum pressure (10−2Torr), whereas Ge xS1-x thin films were prepared by thermal evaporation technique under vacuum (10−5Torr) with (x=0,0.1,0.2 and 0.3). The optical properties measurements shows that the optical energy gap decrease from (3.4 to 3 eV) with the increase of x content, the optical constants declare significant variation with x content variation.