In this study, polyester composites reinforced with pistachio shells powder (P.) with an average
diameter (150 – 200 μm) with different weight ratios (0.5%, 1%, 1.5%, 2%, and 2.5%) were
prepared to the resin. The Shore D hardness, thermal conductivity (K), and the glass transition
temperature (Tg) of the samples were examined. The results showed that the Shore D hardness
increases with the increase of the reinforcement ratio and its maximum value is (87.55) at (2.5%
P.) While the value of hardness at (0%) is (86.5). The thermal conductivity increases slightly with
the increase in the percentage of reinforcement and its maximum value is (0.213253 W/ m. K) at
(2.5% P.), while the value of K at (0% P.) is (0.170264W/ m. K), but with this slight increase in
thermal conductivity, polyester composites remain from the insulating materials. The minimum
(Tg) of (UPE/ P.) composites was the value (113.898°C) at (2.5% P.). Polyester composites are
used in wood paints, either in primitive finishes or final finishes.
The mechanical properties of fiber-reinforced-polymer (FRP)
composites are dependent on the type amount, and orientation of fiber that is selected for a particular service. There are many commercially available reinforcement forms to meet the design requirements of the user. The ability of failure in the fiber architecture allows for optimized performance of a product that saves both weight and cost ( 12).
A modem technology is adopted to produce fibers (glass, kevelar,
and carbon) reinforced composite by using unsaturated polyester, where different volume fraction of these fibers are used (0, 0.2, 0.4, 0.6, 0.8, I)
reinfor
... Show MoreThe change in the optical band gap and optical activation energy have been investigated for pure Poly (vinyl alcohol)and Poly (vinyl alcohol) doped with Aluminum sulphate to proper films from their optical absorption spectra. The absorption spectra were measured in the wave range from (200-700) nm at temperature range (25-140) 0C. The optical band gap (Eg) for allowed direct transition decrease with increase the concentration of Aluminum sulphate. The optical activation energy for allowed direct transition band gap was evaluated using Urbach- edges method. It was found that ?E increases with increasing the concentration of Al2 (SO4)3 and decreases when temperature increases.
The In this experimental study, natural stone powder was utilized to improve a cohesive soil’s compaction and strength properties. According to the significant availability of limestone in the globe, it has been chosen for the purpose of the study, in addition to considering the existing rock industry massive waste. Stone powder was used in percentages of 4, 8, 12, 16% replaced from the soil weight in dry state. Some of cohesive soil’s consistency, shear, and compaction properties were depicted after improvement. The outcomes yielded in significant amendments in the experimented geotechnical properties after stone powder addition considering 60 days curing period. Cohesion and friction angle were notably increased by
... Show MoreStudy the effect of doping V2O5 on polymers poly vinyl alcohol ( PVA), poly vinyl pyrrolidone (PVP) on the optical and structural properties for film prepared by using Casting method at thickness( 300±20)nm ,All the materials dissolved in distilled water by magnetic mixer for one hour .The optical parameters measured by using UV-VIS spectrometer ,and the structural parameters measured by X-ray diffraction .when measured the energy gap found that the value was decreases from 4.6 eV to 2.98 eV with doping .The refractive index ,extinction coefficient ,absorption coefficient ,real and imaginary dielectric constants of (PVA/PVP) are increasing with doping by V2O5 and wit
... Show MoreIn this study, aluminum alloyAA6061-T6 was joined by a hot press process with three types of material; polyamide PA 6.6 (nylon), 1% carbon nanotube/PA6.6 and 30% carbon fiber/PA6.6 composites. Three parameters were considered in the hot pressing; temperature (180, 200 and 220°C), pressure (2, 3, 4, 5 and 6 bar) and time of pressing (1, 2, 3, 4 and 5 minutes for 200ºC, and 0.25, 0.5, 0.75, 1 and 1.25 minutes for220ºC). Applied pressure has great effect on shear strength of the joint, corresponding to bonding time and temperature. Maximum shear strength was 8.89MPa obtained for PA6.6 at bonding conditions of 4 bar, 220ºC and 0.75 minute. For 30% carbon fiber/PA6,6 shear recorded was
This research study the effect of surface modification and copper (Cu) plating carbon fiber (CF) surface on the thermal stability and wettability of carbon fiber (CF)/epoxy (EP) composites. The TGA result indicates that the thermal-stability of carbon fiber may be enhanced after Cu coating CF. TGA curve showed that the treatment temperature was enhanced thermal stability of Ep/CF, this is due to the oxidation during heating. The Cu plating increased the thermal conductivity, this increase might be due to reduce in contact resistance at the interface due to chemical modification and copper plating and tunneling resistance.
The increase of surface polarity after coating cause decreas
... Show MoreIn this research, the effect of reinforcing epoxy resin composites with a filler derived from chopped agriculture waste from oil palm (OP). Epoxy/OP composites were formed by dispersing (1, 3, 5, and 10 wt%) OP filler using a high-speed mechanical stirrer utilizing a hand lay-up method. The effect of adding zinc oxide (ZnO) nanoparticles, with an average size of 10-30 nm, with different wt% (1,2,3, and 5wt%) to the epoxy/oil palm composite, on the behavior of an epoxy/oil palm composite was studied with different ratios (1,2,3, and 5wt%) and an average size of 10-30 nm. Fourier Transform Infrared (FTIR) spectrometry and mechanical properties (tensile, impact, hardness, and wear rate) were used to examine the composites. The FTIR
... Show MoreIn this paper we investigate how do the laminated composites behave mechanically when subjected to external stresses, when reinforced with continuous fibers (mat) and discontinuous fibers (chopped) and to find the effect of the fiber type on the mechanical properties. Laminated composites consisting of wood- wood and Ph-F resin as suitable adhesive were reinforced with different fibers(jute, glass, and carbon).However, two different methods of reinforcement namely, mat and chopped fibers were utilized. The mechanical properties such as (impact strength, compression strength, tensile strength, shear strength, bending strength, and elasticity modulus) of laminated composites were measured. Fibers reinforced laminated composite
... Show MoreThis researchs the preparation of particulate polymer composites from Alkyd resin and Iraqi Burn Kaolin which were added as (20%,30%,40%,50%)and comparing with the polymer. It studied Thermal conductivity and Dielectric strength for both of the Alkyd resin and the Composite Material. The result showed an increase in Dielectric strength after adding the Iraqi Burn Kaolin , also the Thermal conductivity was increased by adding the Iraqi Burn Kaolin .